Direct-Write Lithography Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
→Positive Resist (MLA150): added SPR220-7.0, from Lubin greyscale project
Line 24: Line 24:
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
! width="100" |DeFocus
! width="100" |DeFocus
!Rehydrate
! width="75" |PEB*
! width="75" |PEB*
! width="100" |Developer
! width="100" |Developer
Line 36: Line 37:
|240
|240
|5
|5
|
|''none''
|''none''
|AZ400K:DI 1:4
|AZ400K:DI 1:4
Line 49: Line 51:
|320
|320
|6
|6
|
|''none''
|''none''
|AZ400K:DI 1:4
|AZ400K:DI 1:4
Line 55: Line 58:
|-
|-
|[[Media:AXP4000pb-Datasheet.pdf|AZ4620]]
|[[Media:AXP4000pb-Datasheet.pdf|AZ4620]]
|
|
|
|
|
Line 73: Line 77:
|325
|325
| - 4
| - 4
|
|115°C, 90s
|115°C, 90s
|AZ300MIF
|AZ300MIF
|60s
|60s
|Used HIMT design. 0.6-0.9µm line/space.
|Used HIMT design. 0.6-0.9µm line/space.
|-
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-7.0]]
|3.5 krpm, 30s
|105°C/2min
Cool 1min
|~ 7.0µm
|375
|~550mJ
| -20
|Leave sample to rehydrate for >1hr
|115°C, 90s
|AZ300MiF
|70s
|
|-
|-
|[[Media:SPR955-Positive-Resist-Datasheet.pdf|SPR 955-CM0.9]]
|[[Media:SPR955-Positive-Resist-Datasheet.pdf|SPR 955-CM0.9]]
Line 85: Line 104:
|250
|250
| - 7
| - 7
|
|110°C, 90s
|110°C, 90s
|AZ300MIF
|AZ300MIF
Line 98: Line 118:
|180–220
|180–220
|<nowiki>-4</nowiki>
|<nowiki>-4</nowiki>
|
|100°C, 60s
|100°C, 60s
|AZ300MiF
|AZ300MiF
Line 105: Line 126:
lower dose for clear-field, higher dose for dark-field.
lower dose for clear-field, higher dose for dark-field.
|-
|-
| colspan="11" |*PEB: Post-exposure bake: after exposure, before develop
| colspan="12" |*PEB: Post-exposure bake: after exposure, before develop
|}
|}



Revision as of 20:38, 14 June 2023

Maskless Aligner (Heidelberg MLA150)

Photolithography Recipes for the Heidelberg MLA150. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point.

These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches.

Any I-Line PR is usable, although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR.

Positive Resist (MLA150)

We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies, compensate using CD Bias as described here.

Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus Rehydrate PEB* Developer Developer Time Comments
AZ4110 4 krpm, 30s 95°C, 60s ~ 1.1 µm 405 240 5 none AZ400K:DI 1:4 50s Used HIMT design (good for isolated lines 0.8-1um)
AZ4330 4 krpm, 30s 95°C, 60s ~ 3.3 µm 405 320 6 none AZ400K:DI 1:4 90s Used HIMT design
AZ4620
SPR 220-3.0 2.5 krpm, 30s 115°C, 90s ~ 2.7 µm 405 325 - 4 115°C, 90s AZ300MIF 60s Used HIMT design. 0.6-0.9µm line/space.
SPR 220-7.0 3.5 krpm, 30s 105°C/2min

Cool 1min

~ 7.0µm 375 ~550mJ -20 Leave sample to rehydrate for >1hr 115°C, 90s AZ300MiF 70s
SPR 955-CM0.9 3 krpm, 30s 95°C, 90s ~ 0.9 µm 405 250 - 7 110°C, 90s AZ300MIF 60s Used HIMT design
THMR-3600HP 1.5 krpm, 45s;

250 rpm/s

100°C, 60s 0.430µm 405 180–220 -4 100°C, 60s AZ300MiF 20s ~0.4nm line/space:

lower dose for clear-field, higher dose for dark-field.

*PEB: Post-exposure bake: after exposure, before develop

Negative Resist (MLA150)

We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus PEB* Flood* Developer Developer Time Comments
AZ5214 6 krpm, 30s 95°C, 60s ~ 1.0 µm 375 35 - 5 110°C, 60s 60" AZ300MIF 60s Used UCSB design. Good for up to ~1.3um open line space.
AZnLOF2020 4 krpm, 30s 110°C, 60s ~ 2.1µm 375 340 - 3 110°C, 60s none AZ300MIF 90s Used UCSB design. Good for 2um open line space.
SU-8 2075 ~70µm 375 Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end.
*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal, and requires Flood Exposure with the MA6 or MJB aligner afterwards, before developing.

Greyscale Lithography (MLA150)

AZ4620 is the manufacturer-recommended PR for greyscale litho.

Resist Spin Cond. Bake Thickness Exposure Dose (mJ/cm2) Focus Offset PEB Flood Developer Developer Time Comments
AZ4620 ? krpm/30” 95°C, 60” 60" AZ300MIF 60s
  • TBD