== Nitride2 deposition (PECVD #2) == |
||
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]] |
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]] |
||
*[[media:ADV PECVD NITRIDE2-Data April 2014.pdf|Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate)]] |
*[[media:ADV PECVD NITRIDE2-Data April 2014.pdf|Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate)]] |
||
Revision as of 16:30, 16 April 2014
PECVD 2 (Advanced Vacuum)
Nitride2 deposition (PECVD #2)
- Nitride2 Standard Recipe
- Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate)
- Nitride2 Data April 2014
- Nitride2 Thickness uniformity 2014
- Deposition Rate: ≈ 9.0 nm/min
- Refractive Index: ≈ 1.952
- Stress ≈ 484MPa
SiO2 deposition (PECVD #2)
- Oxide Standard Recipe
- Oxide Data (Deposition Rate, Refractive Index, Stress, HF etch rate )
- Oxide Data April 2014
- Oxide Thickness uniformity 2014
- Deposition Rate: ≈ 28.0 nm/min
- Refractive Index: ≈ 1.472
- Stress ≈ -270MPa
LS SiN deposition (PECVD #2)
- LS Nitride2 Standard Recipe
- LS Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate )
- LS Nitride2 Data April 2014
- LS Nitride2 Thickness uniformity 2014
- Deposition Rate: ≈ 8.34 nm/min
- Refractive Index: ≈ 1.932
- Stress ≈ -45MPa