OLD - PECVD2 Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Biljana (talk | contribs)
Biljana (talk | contribs)
Line 2: Line 2:
== SiN deposition (PECVD #2) ==
== SiN deposition (PECVD #2) ==
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]
*[[media:ADV PECVD NITRIDE2-Data April 2014.pdf|Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate)]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data April 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data April 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]

Revision as of 01:40, 22 May 2014

PECVD 2 (Advanced Vacuum)

SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.29 nm/min
  • Refractive Index: ≈ 1.955
  • Stress ≈ 498MPa
  • HF etch rate:~48nm/min

SiO2 deposition (PECVD #2)

  • Deposition Rate: ≈ 28.0 nm/min
  • Refractive Index: ≈ 1.472
  • Stress ≈ -270MPa

LS SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.34 nm/min
  • Refractive Index: ≈ 1.932
  • Stress ≈ -46MPa

Amorphous-Si deposition (PECVD #2)