OLD - PECVD2 Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Biljana (talk | contribs)
Biljana (talk | contribs)
Line 27: Line 27:
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]


*Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
*Deposition Rate: ≈ 8.14 nm/min (users must calibrate this prior to critical deps)
*Refractive Index: ≈ 1.935
*Refractive Index: ≈ 1.935
*Stress ≈ -0.04MPa
*Stress ≈ -7.18MPa
*HF etch rate~47nm/min
*HF etch rate~48nm/min


== Amorphous-Si deposition (PECVD #2) ==
== Amorphous-Si deposition (PECVD #2) ==

Revision as of 23:00, 1 August 2014

PECVD 2 (Advanced Vacuum)

SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.957
  • Stress ≈ 499MPa
  • HF etch rate:~49nm/min

SiO2 deposition (PECVD #2)

  • Deposition Rate: ≈ 28.50 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.474
  • Stress ≈ -252MPa
  • HF etch rate~616nm/min

LS SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.14 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.935
  • Stress ≈ -7.18MPa
  • HF etch rate~48nm/min

Amorphous-Si deposition (PECVD #2)