OLD - PECVD2 Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
| Line 28: | Line 28: | ||
*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]] |
*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data December 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014] |
||
Revision as of 23:30, 3 December 2014
PECVD 2 (Advanced Vacuum)
Photos
SiN deposition (PECVD #2)
- Deposition Rate: ≈ 7.93 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.961
- Stress ≈ 495MPa
- HF etch rate:~49nm/min
SiO2 deposition (PECVD #2)
- Deposition Rate: ≈ 28.64 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.475
- Stress ≈ -260MPa
- HF etch rate~623nm/min
LS SiN deposition (PECVD #2)
- Deposition Rate: ≈ 7.96 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.937
- Stress ≈ 2.77MPa
- HF etch rate~47nm/min