Dry Etching Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Ningcao (talk | contribs)
No edit summary
m partially alphabetized and removed one spurious row
Line 1: Line 1:
{{Recipe Table Explanation}}
{{Recipe Table Explanation}}
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%"
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%"
|- bgcolor="#D0E7FF"
|- bgcolor="#D0E7FF"
! width="725" height="45" colspan="16" | <div style="font-size: 150%;">Dry Etching Recipes</div>
! colspan="16" width="725" height="45" | <div style="font-size: 150%;">Dry Etching Recipes</div>
|- bgcolor="#D0E7FF"
|- bgcolor="#D0E7FF"
| <!-- INTENTIONALLY LEFT BLANK -->
| <!-- INTENTIONALLY LEFT BLANK -->
! width="300" bgcolor="#D0E7FF" align="center" height="35" colspan="4" | '''[[RIE Etching Recipes|RIE Etching]]'''
! colspan="4" width="300" bgcolor="#D0E7FF" align="center" height="35" | '''[[RIE Etching Recipes|RIE Etching]]'''
! width="300" bgcolor="#D0E7FF" align="center" colspan="4" | '''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="4" width="300" bgcolor="#D0E7FF" align="center" | '''[[ICP Etching Recipes|ICP Etching]]'''
! bgcolor="#D0E7FF" align="center" colspan="4"|'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="4" bgcolor="#D0E7FF" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! bgcolor="#D0E7FF" align="center" colspan="3" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
! colspan="3" bgcolor="#D0E7FF" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
|-
|-
! width="65" bgcolor="#D0E7FF" align="center" | '''Material'''
! width="65" bgcolor="#D0E7FF" align="center" | '''Material'''
Line 26: Line 26:
| width="85" bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| width="85" bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| width="85" bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
| width="85" bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | Al
! bgcolor="#D0E7FF" align="center" | Ag
|
|
|
|
|
|
| [[RIE Etching Recipes|A]]
|
|
⚫
| {{rl|ICP Etching Recipes|Al Etch(Panasonic 1)}}
⚫
| {{rl|ICP Etching Recipes|Al Etch(Panasonic 2)}}
|
|
|
|
Line 40: Line 37:
|
|
|
|
⚫
|
|
|
|
|
⚫
|-
⚫
! bgcolor="#D0E7FF" align="center" | Ti
|
|
|
|
⚫
|
⚫
|
⚫
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | Al
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|Ti Etch(Panasonic 1)}}
| [[RIE Etching Recipes|A]]
⚫
| A
|
|
⚫
| {{rl|ICP Etching Recipes|Al Etch(Panasonic 1)}}
⚫
| {{rl|ICP Etching Recipes|Al Etch(Panasonic 2)}}
|
|
|
|
|
|
|
|
⚫
|
|
|
|
|
⚫
|-bgcolor ="#EEFFFF"
⚫
! bgcolor="#D0E7FF" align="center" | Cr
|
|
|
|
⚫
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | Au
|
|
⚫
| A
|
|
⚫
| {{rl|ICP Etching Recipes|Cr Etch(Panasonic 1)}}
⚫
| A
|
|
|
|
Line 75: Line 70:
|
|
|
|
⚫
|
⚫
|
⚫
|-
⚫
! bgcolor="#D0E7FF" align="center" | Ge
|
|
|
|
Line 84: Line 75:
|
|
|
|
⚫
|
⚫
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
⚫
|- bgcolor="#EEFFFF"
⚫
! bgcolor="#D0E7FF" align="center" | Cr
|
|
|
|
⚫
|
⚫
| A
⚫
|
⚫
| {{rl|ICP Etching Recipes|Cr Etch(Panasonic 1)}}
⚫
| A
|
|
|
|
Line 94: Line 94:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | Ag
! bgcolor="#D0E7FF" align="center" | Cu
|
|
|
|
Line 112: Line 112:
|
|
|-
|-
! bgcolor="#D0E7FF" align="center" | Pt
! bgcolor="#D0E7FF" align="center" | Ge
|
|
|
|
Line 127: Line 127:
|
|
|
|
⚫
|
⚫
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
⚫
|-
⚫
|-bgcolor ="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | Au
! bgcolor="#D0E7FF" align="center" | Ni
|
|
|
|
Line 146: Line 146:
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
|-
! bgcolor="#D0E7FF" align="center" | Ni
! bgcolor="#D0E7FF" align="center" | Pt
|
|
|
|
Line 161: Line 161:
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
|-
⚫
! bgcolor="#D0E7FF" align="center" | Ti
⚫
|-bgcolor ="#EEFFFF"
⚫
! bgcolor="#D0E7FF" align="center" | Cu
⚫
|
⚫
|
|
|
|
|
|
Line 173: Line 169:
|
|
|
|
| {{rl|ICP Etching Recipes|Ti Etch(Panasonic 1)}}
⚫
| A
|
|
|
|
Line 179: Line 177:
|
|
|
|
⚫
|
|
|
|-
|-
Line 197: Line 196:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | Mo
! bgcolor="#D0E7FF" align="center" | Mo
|
|
Line 231: Line 230:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | W-TiW
! bgcolor="#D0E7FF" align="center" | W-TiW
|
|
Line 265: Line 264:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | HfO<sub>2</sub>
! bgcolor="#D0E7FF" align="center" | HfO<sub>2</sub>
|
|
Line 299: Line 298:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | SiO<sub>2</sub>
! bgcolor="#D0E7FF" align="center" | SiO<sub>2</sub>
|
|
Line 333: Line 332:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | SiOxNy
! bgcolor="#D0E7FF" align="center" | SiOxNy
|
|
Line 367: Line 366:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | TiO<sub>2</sub>
! bgcolor="#D0E7FF" align="center" | TiO<sub>2</sub>
|
|
Line 401: Line 400:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | ZnO<sub>2</sub>
! bgcolor="#D0E7FF" align="center" | ZnO<sub>2</sub>
|
|
Line 435: Line 434:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | GaAs
! bgcolor="#D0E7FF" align="center" | GaAs
|
|
Line 469: Line 468:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | InGaAlAs
! bgcolor="#D0E7FF" align="center" | InGaAlAs
|
|
Line 503: Line 502:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | InP
! bgcolor="#D0E7FF" align="center" | InP
|
|
Line 537: Line 536:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | AlGaN
! bgcolor="#D0E7FF" align="center" | AlGaN
|
|
Line 571: Line 570:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
|-
|-
! bgcolor="#D0E7FF" align="center" | GaSb
! bgcolor="#D0E7FF" align="center" | GaSb
Line 589: Line 588:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | CdZnTe
! bgcolor="#D0E7FF" align="center" | CdZnTe
|
|
Line 640: Line 639:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | Si
! bgcolor="#D0E7FF" align="center" | Si
|
|
Line 674: Line 673:
|
|
|
|
|-bgcolor ="#EEFFFF"
|- bgcolor="#EEFFFF"
! bgcolor="#D0E7FF" align="center" | Sapphire
! bgcolor="#D0E7FF" align="center" | Sapphire
|
|