Oxygen Plasma System Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Zwarburg (talk | contribs)
No edit summary
→Ashers (Technics PEII): added SiN etch and chamber clean
Line 1: Line 1:
{{recipes|Dry Etching}}
{{recipes|Dry Etching}}
=[[Ashers (Technics PEII)]]=
==[[Ashers (Technics PEII)]]==

⚫
=[[Plasma Clean (Gasonics 2000)]]=
=== CF4/O2 PEii ===
⚫
=[[UV Ozone Reactor]]=

⚫
=[[Plasma Activation (EVG 810)]]=
==== SiN Etching ====
* Pressure = 300mT–350mT
* Power = 100W
* Etch Rate ≈ 50-100 nm/min. Varies.

=== Chamber Clean after CF4 Etching ===
* Pressure = 300mT–350mT
* Power = 300W
* Time = 10min
* <u>Set power back to 100W ''before'' shutting off plasma!</u>

⚫
==[[Plasma Clean (Gasonics 2000)]]==
⚫
==[[UV Ozone Reactor]]==
⚫
==[[Plasma Activation (EVG 810)]]==

Revision as of 22:25, 28 August 2018

Back to Dry Etching Recipes.

Ashers (Technics PEII)

CF4/O2 PEii

SiN Etching

  • Pressure = 300mT–350mT
  • Power = 100W
  • Etch Rate ≈ 50-100 nm/min. Varies.

Chamber Clean after CF4 Etching

  • Pressure = 300mT–350mT
  • Power = 300W
  • Time = 10min
  • Set power back to 100W before shutting off plasma!

Plasma Clean (Gasonics 2000)

UV Ozone Reactor

Plasma Activation (EVG 810)