*[https://docs.google.com/spreadsheets/d/1uIhx-TD11lDSjpCyPtgKC_CmuNWKLx6iLl5PJgVDt30/edit#gid=sharing Thickness Uniformity SiN 100C 300nm-2019]
*[https://docs.google.com/spreadsheets/d/1uIhx-TD11lDSjpCyPtgKC_CmuNWKLx6iLl5PJgVDt30/edit#gid=sharing Thickness Uniformity SiN 100C 300nm-2019]


=== 2020 Data SiN 250C ===


=== '''2020 Data SiN 250C''' ===
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=sharing SiN 250C 300nm Data-2020]
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=sharing SiN 250C 300nm Data-2020]
*[https://docs.google.com/spreadsheets/d/1UTr93aWx0MjCwVBwRmYjPwo9ASluGQ-OrJhVG_R57aY/edit#gid=sharing SiN 250C Table-2020]
*[https://docs.google.com/spreadsheets/d/1UTr93aWx0MjCwVBwRmYjPwo9ASluGQ-OrJhVG_R57aY/edit#gid=sharing SiN 250C Table-2020]
*[https://docs.google.com/spreadsheets/d/1YAx_Ix84xId8CAhDwZeFT7jLFUwg-BET9aBwg3DxUmQ/edit#gid=sharing Thickness Uniformity SiN 250C 300nm-2020]
*[https://docs.google.com/spreadsheets/d/1YAx_Ix84xId8CAhDwZeFT7jLFUwg-BET9aBwg3DxUmQ/edit#gid=sharing Thickness Uniformity SiN 250C 300nm-2020]


=== 2020 Data SiN LS 250C ===


=== '''2020 Data SiN LS 250C''' ===
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=sharing SiN LS 250C 300nm Data-2020]
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=sharing SiN LS 250C 300nm Data-2020]
*[https://docs.google.com/spreadsheets/d/1MXW7UNpTyk93ucOVQaSun5IX7QaUbSABNHNznb09qw8/edit#gid=sharing SiN LS 250C Table-2020]
*[https://docs.google.com/spreadsheets/d/1MXW7UNpTyk93ucOVQaSun5IX7QaUbSABNHNznb09qw8/edit#gid=sharing SiN LS 250C Table-2020]
Line 238: Line 234:
*[https://docs.google.com/spreadsheets/d/1vYAFwFCWE-bH7iZXXazFyY56vjCcTMIx9fcRJNO115s/edit#gid=sharing SiO2 HDR 100C Table-2019]
*[https://docs.google.com/spreadsheets/d/1vYAFwFCWE-bH7iZXXazFyY56vjCcTMIx9fcRJNO115s/edit#gid=sharing SiO2 HDR 100C Table-2019]
*[https://docs.google.com/spreadsheets/d/1y4mpR4i0gbzSNRbSYGASVSms36FuPh-jDnS3v82OEII/edit#gid=sharing Thickness Uniformity SiO2 HDR 100C 300nm-2019]
*[https://docs.google.com/spreadsheets/d/1y4mpR4i0gbzSNRbSYGASVSms36FuPh-jDnS3v82OEII/edit#gid=sharing Thickness Uniformity SiO2 HDR 100C 300nm-2019]



=== '''2019 Data SiO2 250C''' ===
=== '''2019 Data SiO2 250C''' ===
Line 250: Line 244:
*[https://docs.google.com/spreadsheets/d/1Mm_rsTm9xDQ50kZx6X6EZ5dTegUvinq0zFxRtE8B2R4/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2019]
*[https://docs.google.com/spreadsheets/d/1Mm_rsTm9xDQ50kZx6X6EZ5dTegUvinq0zFxRtE8B2R4/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2019]


=== 2020 Data SiO2 250C ===


=== '''2020 Data SiO2 250C''' ===
*[https://docs.google.com/spreadsheets/d/1bU2Gu3x3DNyrq8skMAQZJCsra-IcoDCT0U5D135YPgc/edit#gid=sharing SiO2 LDR 250C 300nm Data-2020]
*[https://docs.google.com/spreadsheets/d/1bU2Gu3x3DNyrq8skMAQZJCsra-IcoDCT0U5D135YPgc/edit#gid=sharing SiO2 LDR 250C 300nm Data-2020]
*[https://docs.google.com/spreadsheets/d/1T_4gaJQ3wHSNptoAtFR1fN0ePwfw3PsQ0DLSjqGeyM4/edit#gid=sharing SiO2 LDR 250C Table-2020]
*[https://docs.google.com/spreadsheets/d/1T_4gaJQ3wHSNptoAtFR1fN0ePwfw3PsQ0DLSjqGeyM4/edit#gid=sharing SiO2 LDR 250C Table-2020]

Revision as of 21:08, 30 March 2020

Back to Vacuum Deposition Recipes.

PECVD 1 (PlasmaTherm 790)

Historical Particulate Data

SiN deposition (PECVD #1)

Historical Data

Thin-Film Properties
Uniformity Data

SiO2 deposition (PECVD #1)

Historical Data

Thin-Film Properties

Uniformity Data

Low-Stress SiN - LS-SiN (PECVD#1)

SiOxNy deposition (PECVD #1)

Cleaning Recipes (PECVD #1)

To Be Added...

PECVD 2 (Advanced Vacuum)

Historical Particulate Data

SiO2 deposition (PECVD #2)

Standard Recipe

Historical Data

Thin-Film Properties
Uniformity Data

SiN deposition (PECVD #2)

Standard Recipe

Historical Data

Thin-Film Properties
Uniformity Data

Low-Stress SiN deposition (PECVD #2)

Low-Stress SilIcon Nitride (< 100 MPa)

Standard Recipe

Historical Data

Thin-Film Properties
Uniformity Data

Amorphous-Si deposition (PECVD #2)

Cleaning Recipes (PECVD #2)

To Be Added...

ICP-PECVD (Unaxis VLR)

Particulates - historical data

Particulates - 2020

SiN deposition (Unaxis VLR)

The recipe SiN 100C is not valid currently, and is still under development. 
-- Demis 2019-11-22

2020 Data SiN 250C

2020 Data SiN LS 250C

SiO2 deposition (Unaxis VLR)

2019 Data SiO2 100C

2019 Data SiO2 250C

2020 Data SiO2 250C

Cleaning Recipes (Unaxis VLR Dep)

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min