OLD - PECVD2 Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Line 23: Line 23:


*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]
*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]
*[[media:New Advanced PECVD LS NITRIDE2 April 2014.pdf|LS Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate )]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data April 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data April 2014]



Revision as of 01:44, 22 May 2014

PECVD 2 (Advanced Vacuum)

SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.29 nm/min
  • Refractive Index: ≈ 1.955
  • Stress ≈ 498MPa
  • HF etch rate:~48nm/min

SiO2 deposition (PECVD #2)

  • Deposition Rate: ≈ 28.36 nm/min
  • Refractive Index: ≈ 1.473
  • Stress ≈ -256MPa
  • HF etch rate~582nm/min

LS SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.17 nm/min
  • Refractive Index: ≈ 1.935
  • Stress ≈ -0.04MPa
  • HF etch rate~47nm/min

Amorphous-Si deposition (PECVD #2)