OLD - PECVD2 Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
| Line 2: | Line 2: | ||
== SiN deposition (PECVD #2) == |
== SiN deposition (PECVD #2) == |
||
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]] |
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data June 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014] |
||
Revision as of 22:23, 11 June 2014
PECVD 2 (Advanced Vacuum)
SiN deposition (PECVD #2)
- Deposition Rate: ≈ 8.29 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.955
- Stress ≈ 498MPa
- HF etch rate:~48nm/min
SiO2 deposition (PECVD #2)
- Deposition Rate: ≈ 28.36 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.473
- Stress ≈ -256MPa
- HF etch rate~582nm/min
LS SiN deposition (PECVD #2)
- Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.935
- Stress ≈ -0.04MPa
- HF etch rate~47nm/min