== SiN deposition (PECVD #2) ==
== SiN deposition (PECVD #2) ==
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data June 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data July 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]



Revision as of 22:57, 1 August 2014

PECVD 2 (Advanced Vacuum)

SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.957
  • Stress ≈ 499MPa
  • HF etch rate:~49nm/min

SiO2 deposition (PECVD #2)

  • Deposition Rate: ≈ 28.36 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.473
  • Stress ≈ -256MPa
  • HF etch rate~582nm/min

LS SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.935
  • Stress ≈ -0.04MPa
  • HF etch rate~47nm/min

Amorphous-Si deposition (PECVD #2)