Photolithography Recipes for the Heidelberg MLA150.

Positive Resist (MLA150)

General notes: Hotplates used, filters, laser wavelengths, etc.

Resist Spin Cond. Bake Thickness Exposure Time Focus Offset PEB Developer Developer Time Comments
SPR955CM0.9 3 krpm/30” 95°C/60” ~ 0.9 um AZ300MIF

Negative Resist (MLA150)

General notes: Hotplates used, filters, laser wavelengths, etc.

Resist Spin Cond. Bake Thickness Exposure Time Focus Offset PEB Flood Developer Developer Time Comments
AZ5214 6 krpm/30” 95°C/60” ~ 1.0 um 60" AZ300MIF 60"
  • ???