Vacuum Deposition Recipes

From UCSB Nanofab Wiki
Revision as of 21:11, 31 July 2024 by Ffoong (talk | contribs) (Add R level for UNAXIS PECVD)
Jump to navigation Jump to search

Process Control Data

See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.

Deposition Tools/Materials Table

  • R: Recipe is available. Clicking this link will take you to the recipe.
  • A: Material is available for use, but no recipes are provided.
Vacuum Deposition Recipes

E-Beam Evaporation Sputtering Thermal Evaporation Plasma Enhanced Chemical
Vapor Deposition (PECVD)
Atomic Layer Deposition Molecular Vapor Deposition
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 3
(AJA ATC 2000-F)
Sputter 4
(AJA ATC 2200-V)
Sputter 5 (AJA ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAL) Molecular Vapor Deposition (Tool)
Ag A
A A A A








Al A
A A A R1
R1 A A




Al2O3 A A

A R1
R5




R4
AlN



A A
R1




R4
Au A
A A A R1

A A




B














C R1
CeO2
CeO2 deposition (E-Beam 2)












Co A

A R









Cr A

A R


A A




Cu A


R1 A








Fe A

A R









Ge A
A A A A








GeO2 A
Gd A

A










Hf A













HfO2



A A






R4
In








A




Ir A













ITO
ITO deposition (E-Beam 2)

A A
R1






MgF2 A A
MgO A
Mo A


R A








Nb A



R








Nd



A








Ni A
A A R1


A A




NiCr A A
NiFe A A A
Pd A
A A



A A




Pt A
A A A R1 R1





R4
Ru A

A
R






R4
Si
A

R A
R1


R3

SiN



R1 A
R6

R6 R6 R6

SiN - Low Stress R4 R6 R6
SiO2 A A

R1 A A R6

R6 R6 R6 R4
SiOxNy






R3

R4



Sn








A




SrF2
A












Ta A


R1 A
R1






Ta2O5


A


R6






Ti A
A A R1 R1 R1 R1






TiN




R
R1




R4
TiW A


A R1








TiO2
A

A R1
R5




R4
V



A A








W A


A R1








Zn







A A




ZnO












R3
Zr A

A A A








ZrO2












R4
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 3
(ATC 2000-F)
Sputter 4
(ATC 2200-V)
Sputter 5 (ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAl) Molecular Vapor Deposition (Tool)