AZ5214 is a positive PR to start. If you expose and develop, then the exposed areas develop out like a typical positive PR.

Positive operation with NO PEB.

However if instead you expose, then post-exposure-Bake “PEB”, the exposed areas become Hardened/impervious to developer. But the rest of the PR is still unexposed.

So THEN you flood expose the rest of the unexposed PR, and like a positive PR this now allows that PR to develop out.


A Basic 5214 the process should look like:

• Spin + soft-bake

• MLA expose

• P.E.Bake - harden the exposed PR, making it "negative"

• Flood expose - expose the remaining positive PR

• Develop