| colspan="6" |'''InP Ridge Etch''': 60°C, 3mT, 800W/65W, Cl2=18, H2=15, CH4=10sccm, time=5min00sec (300sec) |
| colspan="6" |'''InP Ridge Etch''': 60°C, 3mT, 800W/65W, Cl2=18, H2=15, CH4=10sccm, time=5min00sec (300sec) |
||
Sample Size: 2” unpatterned InP wafer “dummy” pieces, surrounding 1x1cm patterned sample, ~30-40% SiO<sub>2</sub> masking (NingC's pattern). Silicon carrier, no adhesive. |
<u>Sample Size</u>: 2” unpatterned InP wafer “dummy” pieces, surrounding 1x1cm patterned sample, ~30-40% SiO<sub>2</sub> masking (NingC's pattern). Silicon carrier, no adhesive. |
||
Seasoning: 10min “Std Clean - O2/SF6 Chamber Clean 20C (Edit Time)”, then load 2” “dummy” unpatterned InP wafer pieces on Si carrier (rough side up) and run 5min of “Std InP Ridge Etch - Cl2/CH4/H2 60C” |
<u>Seasoning</u>: 10min “Std Clean - O2/SF6 Chamber Clean 20C (Edit Time)”, then load 2” “dummy” unpatterned InP wafer pieces on Si carrier (rough side up) and run 5min of “Std InP Ridge Etch - Cl2/CH4/H2 60C” |
||
<u>Sample Prep</u>: Prior to dry etching, the sample is submerged in NH4OH:DI solution (XYZ:XYZ) for XYZ min, then DI rinsed and N2 dried. |
|||
|- |
|- |
||
!'''Date''' |
!'''Date''' |
||
Line 13: | Line 15: | ||
!'''Comments''' |
!'''Comments''' |
||
!'''SEM Images''' |
!'''SEM Images''' |
||
|- |
|||
|8/1/22 |
|||
|ND_60c_080122 |
|||
|298 |
|||
|9.9 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/2/2e/CS_002.jpg <nowiki>[CS]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/8/82/45D_001.jpg <nowiki>[45D]</nowiki>] |
|||
|- |
|||
|7/1/22 |
|||
|ND_60c_070122 |
|||
|294 |
|||
|11.9 |
|||
|Did not dip in NH4OH |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/6/65/45D_001_8-1-22.jpg <nowiki>[45D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/f/fb/A734DC5E-639E-4FDC-8F30-6F463470BC27.jpeg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|5/19/22 |
|||
|DJ_60c_007 |
|||
|326 |
|||
|TBA |
|||
|After chamber vented, cleaned (wet + dry). Forgot NH<sub>4</sub>OH wet-etch before dry etch. ER and profile look nominal. |
|||
|[[Media:Oxford InP 60C 45DEG02.jpg|[45°1]]],[[Media:Oxford InP 60C 45DEG05.jpg|[45°2]]] |
|||
[[Media:Oxford InP 60C XS05.jpg|[XS]]] |
|||
|- |
|- |
||
|5/11/22 |
|5/11/22 |
||
Line 19: | Line 43: | ||
|9.76 |
|9.76 |
||
| |
| |
||
|[https://wiki.nanotech.ucsb.edu/w/images/2/25/Oxford_60c_10_45D_003.jpg <nowiki>[ |
|[https://wiki.nanotech.ucsb.edu/w/images/2/25/Oxford_60c_10_45D_003.jpg <nowiki>[45°]</nowiki>] |
||
[https://wiki.nanotech.ucsb.edu/w/images/a/aa/Oxford_60c_10_CS_008.jpg <nowiki>[XS]</nowiki>] |
|||
|- |
|- |
||
|5/4/22 |
|5/4/22 |
||
Line 26: | Line 51: | ||
|10.5 |
|10.5 |
||
| |
| |
||
|[https://wiki.nanotech.ucsb.edu/w/images/e/e8/InP_Oxford_60c_09_45D_005.jpg <nowiki>[ |
|[https://wiki.nanotech.ucsb.edu/w/images/e/e8/InP_Oxford_60c_09_45D_005.jpg <nowiki>[45°]</nowiki>] |
||
[https://wiki.nanotech.ucsb.edu/w/images/3/3a/InP_Oxford_60c_09_CS_005.jpg <nowiki>[XS]</nowiki>] |
|||
|- |
|- |
||
|4/27/22 |
|4/27/22 |
||
Line 33: | Line 59: | ||
|9.2 |
|9.2 |
||
|directly after chamber clean. Identical results to before chamber clean. Chamber appeared clean when opened. |
|directly after chamber clean. Identical results to before chamber clean. Chamber appeared clean when opened. |
||
|[https://wiki.nanotech.ucsb.edu/w/images/b/b4/Oxford_60c_08_45D_003.jpg <nowiki>[ |
|[https://wiki.nanotech.ucsb.edu/w/images/b/b4/Oxford_60c_08_45D_003.jpg <nowiki>[45°]</nowiki>] |
||
[https://wiki.nanotech.ucsb.edu/w/images/8/8d/Oxford_60c_08_CS_009.jpg <nowiki>[XS]</nowiki>] |
|||
|- |
|- |
||
|4/26/22 |
|4/26/22 |
||
Line 40: | Line 67: | ||
|9.93 |
|9.93 |
||
|day before chamber clean |
|day before chamber clean |
||
|[https://wiki.nanotech.ucsb.edu/w/images/6/66/Oxford_60c_07_45D_002.jpg <nowiki>[ |
|[https://wiki.nanotech.ucsb.edu/w/images/6/66/Oxford_60c_07_45D_002.jpg <nowiki>[45°]</nowiki>] |
||
[https://wiki.nanotech.ucsb.edu/w/images/2/25/Oxford_60c_07_CS_001.jpg <nowiki>[XS]</nowiki>] |
|||
|- |
|- |
||
|4/19/22 |
|4/19/22 |
||
Line 47: | Line 75: | ||
|9.53 |
|9.53 |
||
|Chamber opened and brown gunk observed in chamber right after the etch was done. Etch rate unaffected. |
|Chamber opened and brown gunk observed in chamber right after the etch was done. Etch rate unaffected. |
||
|[https://wiki.nanotech.ucsb.edu/w/images/0/03/Oxford_60c_06_45D_002.jpg <nowiki>[ |
|[https://wiki.nanotech.ucsb.edu/w/images/0/03/Oxford_60c_06_45D_002.jpg <nowiki>[45°]</nowiki>] |
||
[https://wiki.nanotech.ucsb.edu/w/images/7/7d/Oxford_60c_06_CS_005.jpg <nowiki>[XS]</nowiki>] |
|||
|- |
|- |
||
|4/13/22 |
|4/13/22 |
||
Line 54: | Line 83: | ||
|11.51 |
|11.51 |
||
|New mask pattern with long lines to cleave through. |
|New mask pattern with long lines to cleave through. |
||
|[https://wiki.nanotech.ucsb.edu/w/images/1/12/Oxford_60c_05_45D_004.jpg <nowiki>[ |
|[https://wiki.nanotech.ucsb.edu/w/images/1/12/Oxford_60c_05_45D_004.jpg <nowiki>[45°]</nowiki>] |
||
[https://wiki.nanotech.ucsb.edu/w/images/5/56/Oxford_60c_05_CS_002.jpg <nowiki>[XS]</nowiki>] |
|||
|- |
|- |
||
! |
! |
||
Line 69: | Line 99: | ||
|*etched for 3min* |
|*etched for 3min* |
||
~30-40% SiO<sub>2</sub> masking (NingC's pattern) |
~30-40% SiO<sub>2</sub> masking (NingC's pattern) |
||
|[https://wiki.nanotech.ucsb.edu/w/images/8/8a/Oxford_60c_04_45D_001.jpg <nowiki>[ |
|[https://wiki.nanotech.ucsb.edu/w/images/8/8a/Oxford_60c_04_45D_001.jpg <nowiki>[45°]</nowiki>] |
||
[https://wiki.nanotech.ucsb.edu/w/images/0/0a/Oxford_60c_04_CS_004.jpg <nowiki>[XS]</nowiki>] |
|||
|- |
|- |
||
|1/26/22 |
|1/26/22 |
||
Line 76: | Line 107: | ||
|12.9 |
|12.9 |
||
|~30-40% SiO<sub>2</sub> masking (NingC's pattern) |
|~30-40% SiO<sub>2</sub> masking (NingC's pattern) |
||
|[https://wiki.nanotech.ucsb.edu/w/images/e/ef/Oxford_Cal_01_26_22_003New_45d_001.jpg <nowiki>[ |
|[https://wiki.nanotech.ucsb.edu/w/images/e/ef/Oxford_Cal_01_26_22_003New_45d_001.jpg <nowiki>[45°]</nowiki>] |
||
[https://wiki.nanotech.ucsb.edu/w/images/4/40/Oxford_Cal_01_26_22_031New_CS_001.jpg <nowiki>[XS]</nowiki>] |
|||
|} |
|} |
||
Revision as of 00:25, 13 August 2022
Data - InP Ridge Etch (Oxford ICP Etcher)
PECVD SiO2 hardmask, patterned on Stepper #2 (AutoStep 200) & Panasonic ICP #1
InP Ridge Etch: 60°C, 3mT, 800W/65W, Cl2=18, H2=15, CH4=10sccm, time=5min00sec (300sec)
Sample Size: 2” unpatterned InP wafer “dummy” pieces, surrounding 1x1cm patterned sample, ~30-40% SiO2 masking (NingC's pattern). Silicon carrier, no adhesive. Seasoning: 10min “Std Clean - O2/SF6 Chamber Clean 20C (Edit Time)”, then load 2” “dummy” unpatterned InP wafer pieces on Si carrier (rough side up) and run 5min of “Std InP Ridge Etch - Cl2/CH4/H2 60C” Sample Prep: Prior to dry etching, the sample is submerged in NH4OH:DI solution (XYZ:XYZ) for XYZ min, then DI rinsed and N2 dried. | |||||
Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (InP/SiO2) | Comments | SEM Images |
---|---|---|---|---|---|
8/1/22 | ND_60c_080122 | 298 | 9.9 | [CS] [45D] | |
7/1/22 | ND_60c_070122 | 294 | 11.9 | Did not dip in NH4OH | [45D] [CS] |
5/19/22 | DJ_60c_007 | 326 | TBA | After chamber vented, cleaned (wet + dry). Forgot NH4OH wet-etch before dry etch. ER and profile look nominal. | [45°1],[45°2] |
5/11/22 | NP_60c_010 | 322 | 9.76 | [45°] | |
5/4/22 | NP_60c_009 | 318 | 10.5 | [45°] | |
4/27/22 | NP_60c_008 | 320 | 9.2 | directly after chamber clean. Identical results to before chamber clean. Chamber appeared clean when opened. | [45°] |
4/26/22 | NP_60c_007 | 312 | 9.93 | day before chamber clean | [45°] |
4/19/22 | NP_60c_006 | 330 | 9.53 | Chamber opened and brown gunk observed in chamber right after the etch was done. Etch rate unaffected. | [45°] |
4/13/22 | NP_60c_005 | 320 | 11.51 | New mask pattern with long lines to cleave through. | [45°] |
↑ Changed mask pattern going forward (~50% open area), apparent etch rate changes due to measuring different features. | |||||
3/30/22 | NP_60c_004 | 427 | 11.17 | *etched for 3min*
~30-40% SiO2 masking (NingC's pattern) |
[45°] |
1/26/22 | NP_1_26_003 | 452 | 12.9 | ~30-40% SiO2 masking (NingC's pattern) | [45°] |
Dependence on Sample Size
We have found that the size of the InP piece loaded (no adhesive, onto Silicon carrier wafer) affects the etch rate, but does not affect the etch profile - ie. etches are still smooth and vertical, but rate varies with sample area.
InP Ridge Etch: 60°C, 3mT, 800W/65W, Cl2=18, H2=15, CH4=10sccm, time=5min05sec (305sec)
Silicon carrier, no adhesive. | |||||||
Date | Sample# | Sample Size (dimensions, mm) | Sample Size (area, mm2) | Etch Rate (nm/min) | Etch Selectivity (InP/SiO2) | Comments | SEM Images |
---|---|---|---|---|---|---|---|
1/11/22 | DJ_InPRidge | 4.5 x 2.5 | 11.25 | 602 | 64.6nm left | ~50% SiO2 masking (GCA Calibration pattern) | [1] |
1/12/22 | DJ_InPRidge | 4.5 x 3 | 13.5 | 563 | 76.4nm left | ~50% SiO2 masking (GCA Calibration pattern) | [2] |
1/12/22 | DJ_InP#3 | 4.5 x 3 | 13.5 | 612 | 71nm left | ~50% SiO2 masking (GCA Calibration pattern) | [3] |
1/26/22 | NP_? | 10 x 10 | 100 | 400-450 | ~250nm left | ~30-40% SiO2 masking (NingC's pattern) | |
1/26/22 | NP_? | 1/4 of 50mm wafer | 490 | 378 | 276nm left | ~30-40% SiO2 masking (NingC's pattern) | [1] |