(link to recipes) |
|||
Line 10: | Line 10: | ||
#*Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving. | #*Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving. | ||
#*Pump down. | #*Pump down. | ||
− | #*Load the deposition recipe (STD SiO2), and run it. Deposition time is variable. Get the rate from [https://wiki.nanotech.ucsb.edu/wiki/ | + | #*Load the deposition recipe (STD SiO2), and run it. Deposition time is variable. Get the rate from [https://wiki.nanotech.ucsb.edu/wiki/PECVD_2_(Advanced_Vacuum) historical data]. |
#*Unload the wafer. | #*Unload the wafer. | ||
#Cleaning | #Cleaning |
Revision as of 16:53, 22 April 2020
There are three standard recipes : STD SiO2, STD Nitride2, and STD LS Nitride2 at 300C. Instructions bellow explain how to run each of the recipes ( seasoning, deposition, cleaning)
Standard Oxide Deposition
STD SiO2
- Log in to Advanced PECVD #2
- Seasoning
- Load the seasoning recipe (STD SiO2), and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (STD SiO2), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning.
- Log out
Standard Nitride Deposition
STD Nitride2
- Log in to Advanced PECVD #2
- Seasoning
- Load the seasoning recipe (STD Nitride2), and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (STD Nitride2), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning.
- Log out
Standard Low Stress Deposition
STD LS Nitride2
- Log in to Advanced PECVD #2
- Seasoning
- Load the seasoning recipe (STD LS Nitride2), and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (STD LS Nitride2), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning.
- Log out