==Materials Table== |
|||
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable" |
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable" |
||
|- |
|- |
||
! colspan=8 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table</div> |
! colspan=8 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table for Thermal Evaporator #1</div> |
||
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
! width="45" bgcolor="#D0E7FF" align="center" | '''Material''' |
! width="45" bgcolor="#D0E7FF" align="center" | '''Material''' |
||
! width="45" bgcolor="#D0E7FF" align="center" | '''Symbol''' |
! width="45" bgcolor="#D0E7FF" align="center" | '''Symbol''' |
||
! width=" |
! width="95" bgcolor="#D0E7FF" align="center" | '''Density, g/cm3''' |
||
! width="45" bgcolor="#D0E7FF" align="center" | '''Z Ratio''' |
! width="45" bgcolor="#D0E7FF" align="center" | '''Z Ratio''' |
||
! width="45" bgcolor="#D0E7FF" align="center" | '''Tooling, %''' |
! width="45" bgcolor="#D0E7FF" align="center" | '''Tooling, %''' |
||
! width=" |
! width="95" bgcolor="#D0E7FF" align="center" | '''Current, Amp''' |
||
! width=" |
! width="95" bgcolor="#D0E7FF" align="center" | '''Dep.rate, A/sec''' |
||
! width=" |
! width="95" bgcolor="#D0E7FF" align="center" | '''Comments''' |
||
|- |
|- |
||
|Aluminum |
|Aluminum |
||
| Line 26: | Line 29: | ||
|Chromium |
|Chromium |
||
|Cr |
|Cr |
||
| |
|7.20 |
||
| |
|28.95 |
||
|95 |
|95 |
||
|85 |
|85 |
||
| Line 177: | Line 180: | ||
| |
| |
||
|- |
|- |
||
|Strontium Fluoride |
|||
|StrontiumFluoride |
|||
|SrF<sub>2 |
|SrF<sub>2 |
||
|4.28 |
|4.28 |
||
|12.15 |
|12.15 |
||
| Line 196: | Line 199: | ||
|- |
|- |
||
|ITO(IndiumTinOxide) |
|ITO(IndiumTinOxide) |
||
|In<sub>2</sub>O<sub>3</sub> - |
|In<sub>2</sub>O<sub>3</sub> - SnO<sub>2 |
||
|6.43-7.14 |
|6.43-7.14 |
||
|0.841 |
|0.841 |
||
| Line 204: | Line 207: | ||
| |
| |
||
|- |
|- |
||
|Permalloy |
|Permalloy |
||
|Ni<sub>0.1</sub>Fe<sub>0.2 |
|Ni<sub>0.1</sub>Fe<sub>0.2</sub> |
||
|8.7 |
|8.7 |
||
|26.40 |
|26.40 |
||
| Line 212: | Line 215: | ||
|0.1 |
|0.1 |
||
| |
| |
||
|} |
|||
=[[Thermal Evaporator 2]]= |
|||
== Materials Table == |
|||
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable" |
|||
|- |
|- |
||
! colspan=6 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table for Thermal Evaporator #2</div> |
|||
|- bgcolor="#D0E7FF" |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Material''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Symbol''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Density, g/cm3''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Z Ratio''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Tooling, %''' |
|||
! width="100" bgcolor="#D0E7FF" align="center" | '''Comments''' |
|||
|- |
|||
|Aluminum |
|||
|Al |
|||
|2.70 |
|||
|1.08 |
|||
| |
|||
| |
|||
|- |
|||
|Antimony |
|||
|Sb |
|||
|6.620 |
|||
|0.768 |
|||
| |
|||
| |
|||
|- |
|||
|Arsenic |
|||
|As |
|||
|5.73 |
|||
|0.996 |
|||
| |
|||
| |
|||
|- |
|||
|Beryllium |
|||
|Be |
|||
|1.85 |
|||
|0.543 |
|||
| |
|||
| |
|||
|- |
|||
|Boron |
|||
|B |
|||
|2.54 |
|||
|0.389 |
|||
| |
|||
| |
|||
|- |
|||
|Cadmium |
|||
|Cd |
|||
|8.64 |
|||
|0.682 |
|||
| |
|||
| |
|||
|- |
|||
|Cadmium sulfide |
|||
|CdS |
|||
|4.83 |
|||
|1.02 |
|||
| |
|||
| |
|||
|- |
|||
|Cadmium telluride |
|||
|CdTe |
|||
|5.85 |
|||
|0.980 |
|||
| |
|||
| |
|||
|- |
|||
|Calcium fluoride |
|||
|CaF<sub>2</sub> |
|||
|3.18 |
|||
|0.775 |
|||
| |
|||
|Used often |
|||
|- |
|||
|Carbon (graphite) |
|||
|C |
|||
|2.25 |
|||
|3.26 |
|||
| |
|||
| |
|||
|- |
|||
|Chromium |
|||
|Cr |
|||
|7.20 |
|||
|0.305 |
|||
|155 |
|||
|Used often |
|||
|- |
|||
|Cobalt |
|||
|Co |
|||
|8.71 |
|||
|0.343 |
|||
| |
|||
| |
|||
|- |
|||
|Copper |
|||
|Cu |
|||
|8.93 |
|||
|0.437 |
|||
| |
|||
| |
|||
|- |
|||
|Gallium |
|||
|Ga |
|||
|5.93 |
|||
|0.593 |
|||
| |
|||
| |
|||
|- |
|||
|Gallium Arsenide |
|||
|GaAs |
|||
|5.31 |
|||
|1.59 |
|||
| |
|||
| |
|||
|- |
|||
|Germanium |
|||
|Ge |
|||
|5.35 |
|||
|0.516 |
|||
| |
|||
| |
|||
|- |
|||
|Gold |
|||
|Au |
|||
|19.30 |
|||
|0.381 |
|||
| |
|||
|Used often |
|||
|- |
|||
|Indium |
|||
|In |
|||
|7.30 |
|||
|0.841 |
|||
|120 |
|||
|Used often |
|||
|- |
|||
|Indium antimonide |
|||
|InSb |
|||
|5.76 |
|||
|0.769 |
|||
| |
|||
| |
|||
|- |
|||
|Iridium |
|||
|Ir |
|||
|22.4 |
|||
|0.129 |
|||
| |
|||
| |
|||
|- |
|||
|Iron |
|||
|Fe |
|||
|7.86 |
|||
|0.349 |
|||
| |
|||
| |
|||
|- |
|||
|Lead |
|||
|Pb |
|||
|11.3 |
|||
|1.13 |
|||
| |
|||
| |
|||
|- |
|||
|Lead sulfide |
|||
|PbS |
|||
|7.50 |
|||
|0.566 |
|||
| |
|||
| |
|||
|- |
|||
|Lithium fluoride |
|||
|LiF |
|||
|2.638 |
|||
|0.778 |
|||
| |
|||
| |
|||
|- |
|||
|Magnesium |
|||
|Mg |
|||
|1.74 |
|||
|1.61 |
|||
| |
|||
| |
|||
|- |
|||
|Magnesium oxide |
|||
|MgO |
|||
|3.58 |
|||
|0.411 |
|||
| |
|||
| |
|||
|- |
|||
|Magnesium Fluoride |
|||
|MgF<sub>2</sub> |
|||
|3.00 ( should be 3.18) |
|||
|0.427( should be 0.637) |
|||
| |
|||
| |
|||
|- |
|||
|Manganese |
|||
|Mn |
|||
|7.20 |
|||
|0.377 |
|||
| |
|||
| |
|||
|- |
|||
|Manganese(II) Sulfide |
|||
|MnS |
|||
|3.99 |
|||
|0.94 |
|||
| |
|||
| |
|||
|- |
|||
|Mercury |
|||
|Hg |
|||
|13.46 |
|||
|0.74 |
|||
| |
|||
| |
|||
|- |
|||
|Molybdenum |
|||
|Mo |
|||
|10.2 |
|||
|0.257 |
|||
| |
|||
| |
|||
|- |
|||
|Nickel |
|||
|Ni |
|||
|8.91 |
|||
|0.331 |
|||
| |
|||
|Used often |
|||
|- |
|||
|Niobium |
|||
|Nb |
|||
|8.578 |
|||
|0.492 |
|||
| |
|||
| |
|||
|- |
|||
|Niobium(V) Oxide |
|||
|Nb<sub>2</sub>O<sub>5</sub> |
|||
|4.47 |
|||
|*1.00 |
|||
| |
|||
|*z ratio has not been established |
|||
|- |
|||
|Palladium |
|||
|Pd |
|||
|12.0 |
|||
|0.357 |
|||
| |
|||
| |
|||
|- |
|||
|Platinum |
|||
|Pt |
|||
|21.4 |
|||
|0.245 |
|||
| |
|||
| |
|||
|- |
|||
|Potasium Cloride |
|||
|KCl |
|||
|1.98 |
|||
|2.05 |
|||
| |
|||
| |
|||
|- |
|||
|Selenium |
|||
|Se |
|||
|4.82 |
|||
|0.864 |
|||
| |
|||
| |
|||
|- |
|||
|Silicon |
|||
|Si |
|||
|2.32 |
|||
|0.712 |
|||
| |
|||
| |
|||
|- |
|||
|Silicon(II) Oxide |
|||
|SiO |
|||
|2.13 |
|||
|0.87 |
|||
| |
|||
| |
|||
|- |
|||
|Silicon dioxide (fused quarz) |
|||
|SiO<sub>2</sub> |
|||
|2.20 |
|||
|1.07 |
|||
| |
|||
| |
|||
|- |
|||
|Silver |
|||
|Ag |
|||
|10.5 |
|||
|0.529 |
|||
| |
|||
| |
|||
|- |
|||
|Silver bromide |
|||
|AgBr |
|||
|6.47 |
|||
|1.18 |
|||
| |
|||
| |
|||
|- |
|||
|Silver chloride |
|||
|AgCl |
|||
|5.56 |
|||
|1.32 |
|||
| |
|||
| |
|||
|- |
|||
|Sodium |
|||
|Na |
|||
|0.97 |
|||
|4.8 |
|||
| |
|||
| |
|||
|- |
|||
|Sodium chloride |
|||
|NaCl |
|||
|2.17 |
|||
|1.57 |
|||
| |
|||
| |
|||
|- |
|||
|Tantalum |
|||
|Ta |
|||
|16.6 |
|||
|0.262 |
|||
| |
|||
| |
|||
|- |
|||
|Tantalum(IV) oxide |
|||
|Ta<sub>2</sub>O<sub>5</sub> |
|||
|8.2 |
|||
|0.30 |
|||
| |
|||
| |
|||
|- |
|||
|Tin |
|||
|Sn |
|||
|7.30 |
|||
|0.724 |
|||
| |
|||
|Used often |
|||
|- |
|||
|Titanium |
|||
|Ti |
|||
|4.50 |
|||
|0.628 |
|||
| |
|||
|Used often |
|||
|- |
|||
|Titanium (IV) Oxide |
|||
|TiO<sub>2</sub> |
|||
|4.26 |
|||
|0.40 |
|||
| |
|||
| |
|||
|- |
|||
|Titanium Oxide |
|||
|TiO |
|||
|4.90 |
|||
|*1.00 |
|||
| |
|||
|* z ratio not established |
|||
|- |
|||
|Tungsten |
|||
|W |
|||
|19.3 |
|||
|0.163 |
|||
| |
|||
| |
|||
|- |
|||
|Tungsten carbide |
|||
|WC |
|||
|15.6 |
|||
|0.151 |
|||
| |
|||
| |
|||
|- |
|||
|Zinc |
|||
|Zn |
|||
|7.04 |
|||
|0.514 |
|||
| |
|||
|Used often |
|||
|- |
|||
|Zinc Oxide |
|||
|ZnO |
|||
|5.61 |
|||
|0.556 |
|||
| |
|||
| |
|||
|- |
|||
|Zinc Sulfide |
|||
|ZnS |
|||
|4.09 |
|||
|0.775 |
|||
| |
|||
| |
|||
|- |
|||
|Zirconium |
|||
|Zr |
|||
|6.51 |
|||
|0.60 |
|||
| |
|||
|Should be 6.49 |
|||
|- |
|||
|Zirconium Oxide |
|||
|ZrO<sub>2</sub> |
|||
|5.6 |
|||
|1.001 |
|||
| |
|||
| |
|||
|} |
|||
== In Deposition (Thermal Evaporator 2) == |
|||
= Materials Table = |
|||
*[[media:Thermal evaporator 2-new Sheet1.pdf|Indium evaporation Data]] |
|||
Revision as of 00:00, 27 June 2018
Back to Vacuum Deposition Recipes.
Thermal Evaporator 1
Materials Table
Materials Table for Thermal Evaporator #1
| |||||||
|---|---|---|---|---|---|---|---|
| Material | Symbol | Density, g/cm3 | Z Ratio | Tooling, % | Current, Amp | Dep.rate, A/sec | Comments |
| Aluminum | Al | 2.70 | 8.17 | 95 | 85 | 1 | Used often |
| Chromium | Cr | 7.20 | 28.95 | 95 | 85 | 2 | Used often |
| Cobalt | Co | 8.71 | 25.74 | ||||
| Copper | Cu | 8.93 | 20.21 | 100 | Used often | ||
| Gold | Au | 19.32 | 23.18 | 101.2 | 122 | 5 | Used often |
| Gold/Palladium | Au.5/Pd.5 | 15.86 | 23.96 | ||||
| Gold/Palladium | Au.5/Pd.4 | 16.40 | 23.80 | ||||
| Gold/Zinc | Au.95/Zn.05 | 18.72 | 22.89 | 101.2 | |||
| Gold/Zinc | Au.90/Zn.10 | 18.07 | 22.58 | ||||
| Magnezium | Mg | 1.74 | 5.48 | 98.4 | |||
| Manganese | Mn | 7.20 | 23.40 | 120 | 100 | ||
| Nickel | Ni | 8.90 | 26.68 | 100 | 50 | 4.5 | Used often |
| Nichrome | NiCr | 8.32 | 27.59 | 100 | 0.4 | ||
| Palladium | Pd | 12.40 | 24.73 | 140.5 | 62 | 1.5 | Used often |
| Silicon Monoxide | SiO | 2.13 | 10.19 | 120 | 70 | ||
| Silver | Ag | 10.5 | 16.69 | ||||
| Zinc | Zn | 7.14 | 17.18 | 50 | 4.5 | Used often | |
| Zinc Oxide | ZnO | 5.61 | 15.88 | ||||
| Strontium Fluoride | SrF2 | 4.28 | 12.15 | 200 | |||
| Iron | Fe | 7.86 | 25.30 | ||||
| ITO(IndiumTinOxide) | In2O3 - SnO2 | 6.43-7.14 | 0.841 | ||||
| Permalloy | Ni0.1Fe0.2 | 8.7 | 26.40 | 140 | 0.1 | ||
Thermal Evaporator 2
Materials Table
Materials Table for Thermal Evaporator #2
| |||||
|---|---|---|---|---|---|
| Material | Symbol | Density, g/cm3 | Z Ratio | Tooling, % | Comments |
| Aluminum | Al | 2.70 | 1.08 | ||
| Antimony | Sb | 6.620 | 0.768 | ||
| Arsenic | As | 5.73 | 0.996 | ||
| Beryllium | Be | 1.85 | 0.543 | ||
| Boron | B | 2.54 | 0.389 | ||
| Cadmium | Cd | 8.64 | 0.682 | ||
| Cadmium sulfide | CdS | 4.83 | 1.02 | ||
| Cadmium telluride | CdTe | 5.85 | 0.980 | ||
| Calcium fluoride | CaF2 | 3.18 | 0.775 | Used often | |
| Carbon (graphite) | C | 2.25 | 3.26 | ||
| Chromium | Cr | 7.20 | 0.305 | 155 | Used often |
| Cobalt | Co | 8.71 | 0.343 | ||
| Copper | Cu | 8.93 | 0.437 | ||
| Gallium | Ga | 5.93 | 0.593 | ||
| Gallium Arsenide | GaAs | 5.31 | 1.59 | ||
| Germanium | Ge | 5.35 | 0.516 | ||
| Gold | Au | 19.30 | 0.381 | Used often | |
| Indium | In | 7.30 | 0.841 | 120 | Used often |
| Indium antimonide | InSb | 5.76 | 0.769 | ||
| Iridium | Ir | 22.4 | 0.129 | ||
| Iron | Fe | 7.86 | 0.349 | ||
| Lead | Pb | 11.3 | 1.13 | ||
| Lead sulfide | PbS | 7.50 | 0.566 | ||
| Lithium fluoride | LiF | 2.638 | 0.778 | ||
| Magnesium | Mg | 1.74 | 1.61 | ||
| Magnesium oxide | MgO | 3.58 | 0.411 | ||
| Magnesium Fluoride | MgF2 | 3.00 ( should be 3.18) | 0.427( should be 0.637) | ||
| Manganese | Mn | 7.20 | 0.377 | ||
| Manganese(II) Sulfide | MnS | 3.99 | 0.94 | ||
| Mercury | Hg | 13.46 | 0.74 | ||
| Molybdenum | Mo | 10.2 | 0.257 | ||
| Nickel | Ni | 8.91 | 0.331 | Used often | |
| Niobium | Nb | 8.578 | 0.492 | ||
| Niobium(V) Oxide | Nb2O5 | 4.47 | *1.00 | *z ratio has not been established | |
| Palladium | Pd | 12.0 | 0.357 | ||
| Platinum | Pt | 21.4 | 0.245 | ||
| Potasium Cloride | KCl | 1.98 | 2.05 | ||
| Selenium | Se | 4.82 | 0.864 | ||
| Silicon | Si | 2.32 | 0.712 | ||
| Silicon(II) Oxide | SiO | 2.13 | 0.87 | ||
| Silicon dioxide (fused quarz) | SiO2 | 2.20 | 1.07 | ||
| Silver | Ag | 10.5 | 0.529 | ||
| Silver bromide | AgBr | 6.47 | 1.18 | ||
| Silver chloride | AgCl | 5.56 | 1.32 | ||
| Sodium | Na | 0.97 | 4.8 | ||
| Sodium chloride | NaCl | 2.17 | 1.57 | ||
| Tantalum | Ta | 16.6 | 0.262 | ||
| Tantalum(IV) oxide | Ta2O5 | 8.2 | 0.30 | ||
| Tin | Sn | 7.30 | 0.724 | Used often | |
| Titanium | Ti | 4.50 | 0.628 | Used often | |
| Titanium (IV) Oxide | TiO2 | 4.26 | 0.40 | ||
| Titanium Oxide | TiO | 4.90 | *1.00 | * z ratio not established | |
| Tungsten | W | 19.3 | 0.163 | ||
| Tungsten carbide | WC | 15.6 | 0.151 | ||
| Zinc | Zn | 7.04 | 0.514 | Used often | |
| Zinc Oxide | ZnO | 5.61 | 0.556 | ||
| Zinc Sulfide | ZnS | 4.09 | 0.775 | ||
| Zirconium | Zr | 6.51 | 0.60 | Should be 6.49 | |
| Zirconium Oxide | ZrO2 | 5.6 | 1.001 | ||