Contact Alignment Recipes: Difference between revisions
(added some of the PR datasheet links) |
(→Negative Resist (MA-6): subheading for SU8) |
||
(3 intermediate revisions by the same user not shown) | |||
Line 30: | Line 30: | ||
! width="300" |Comments |
! width="300" |Comments |
||
|- |
|- |
||
|[[Media:AXP4000pb-Datasheet.pdf|AZ4110]] |
|||
|AZ4110 |
|||
|4 krpm/30” |
|4 krpm/30” |
||
|95°C/60” |
|95°C/60” |
||
Line 39: | Line 39: | ||
| align="left" | |
| align="left" | |
||
|- |
|- |
||
|[[Media:AXP4000pb-Datasheet.pdf|AZ4210]] |
|||
|AZ4210 |
|||
|4 krpm/30” |
|4 krpm/30” |
||
|95°C/60” |
|95°C/60” |
||
Line 70: | Line 70: | ||
|- |
|- |
||
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR220-7.0]] |
|||
|SPR220-7.0 |
|||
|3.5 krpm/45” |
|3.5 krpm/45” |
||
|115°C/120” |
|115°C/120” |
||
Line 92: | Line 92: | ||
! width="100" |Thickness |
! width="100" |Thickness |
||
! width="125" |Exposure Time |
! width="125" |Exposure Time |
||
! width="100" |PEB |
! width="100" |PEB* |
||
! width="100" |Flood |
! width="100" |Flood** |
||
! width="125" |Developer |
! width="125" |Developer |
||
! width="125" |Developer Time |
! width="125" |Developer Time |
||
! width="350" |Comments |
! width="350" |Comments |
||
|- |
|- |
||
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]] |
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]]** |
||
|6 krpm/30” |
|6 krpm/30” |
||
|95°C/60” |
|95°C/60” |
||
Line 111: | Line 111: | ||
|- |
|- |
||
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]] |
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]]** |
||
|6 krpm/30” |
|6 krpm/30” |
||
|95°C/60” |
|95°C/60” |
||
Line 124: | Line 124: | ||
|- |
|- |
||
|[[Media:AZnLOF2020-Negative-Resist-Datasheet.pdf|AZnLOF2020]] |
|||
|AZnLOF2020 |
|||
|3 krpm/30” |
|3 krpm/30” |
||
|110°C/90” |
|110°C/90” |
||
Line 139: | Line 139: | ||
|- |
|- |
||
|NR9-6000PY |
|[[Media:NR9-6000PY-revA.pdf|NR9-6000PY]] |
||
|3 krpm/30” |
|3 krpm/30” |
||
|140°C/180” |
|140°C/180” |
||
Line 151: | Line 151: | ||
*Before litho, do Gasonics #3, 120"; Bake at 140 C, 5' |
*Before litho, do Gasonics #3, 120"; Bake at 140 C, 5' |
||
*Spin-on HMDS 3krpm 30", prior to NR9-6000PY |
*Spin-on HMDS 3krpm 30", prior to NR9-6000PY |
||
|- |
|||
| colspan="10" |*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal |
|||
<nowiki>**</nowiki> To use AZ5214 as a negative PR requires Flood Exposure with the [[Contact Aligner (SUSS MA-6)|MA6]] or [[Suss Aligners (SUSS MJB-3)|MJB]] aligner '''''after PEB''''', before developing. See here for a [[AZ5214 - Basic Process|basic AZ5214 process]], it is different than typical negative resists. |
|||
|} |
|} |
||
Line 172: | Line 174: | ||
! width="300" |Comments |
! width="300" |Comments |
||
|- |
|- |
||
|[[Media:AXP4000pb-Datasheet.pdf|AZ4110]] |
|||
|AZ4110 |
|||
|4 krpm/30” |
|4 krpm/30” |
||
|95°C/60” |
|95°C/60” |
||
Line 181: | Line 183: | ||
| align="left" | |
| align="left" | |
||
|- |
|- |
||
|[[Media:AXP4000pb-Datasheet.pdf|AZ4210]] |
|||
|AZ4210 |
|||
|4 krpm/30” |
|4 krpm/30” |
||
|95°C/60” |
|95°C/60” |
||
Line 221: | Line 223: | ||
|- |
|- |
||
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR220-7.0]] |
|||
|SPR220-7.0 |
|||
|3.5 krpm/45” |
|3.5 krpm/45” |
||
|115°C/120” |
|115°C/120” |
||
Line 243: | Line 245: | ||
! width="100" |Thickness |
! width="100" |Thickness |
||
! width="125" |Exposure Time |
! width="125" |Exposure Time |
||
! width="100" |PEB |
! width="100" |PEB* |
||
! width="100" |Flood Exposure |
! width="100" |Flood Exposure** |
||
! width="125" |Developer |
! width="125" |Developer |
||
! width="125" |Developer Time |
! width="125" |Developer Time |
||
! width="350" |Comments |
! width="350" |Comments |
||
|- |
|- |
||
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]] |
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]]** |
||
|6 krpm/30” |
|6 krpm/30” |
||
|95°C/60” |
|95°C/60” |
||
Line 262: | Line 264: | ||
|- |
|- |
||
|[[Media:AZnLOF2020-Negative-Resist-Datasheet.pdf|AZnLOF2020]] |
|||
|AZnLOF2020 |
|||
|3 krpm/30” |
|3 krpm/30” |
||
|110°C/90” |
|110°C/90” |
||
Line 275: | Line 277: | ||
|- |
|- |
||
|[[Media:AZnLOF2020-Negative-Resist-Datasheet.pdf|AZnLOF2035]] |
|||
|AZnLOF2035 |
|||
|2.5 krpm/30” |
|2.5 krpm/30” |
||
|110°C/60” |
|110°C/60” |
||
Line 288: | Line 290: | ||
|- |
|- |
||
|NR9-6000PY |
|[[Media:NR9-6000PY-revA.pdf|NR9-6000PY]] |
||
|3 krpm/30” |
|3 krpm/30” |
||
|140°C/180” |
|140°C/180” |
||
Line 300: | Line 302: | ||
*Before litho, do Gasonics #3, 120"; Bake at 140 C, 5' |
*Before litho, do Gasonics #3, 120"; Bake at 140 C, 5' |
||
*Spin-on HMDS 3krpm 30", prior to NR9-6000PY |
*Spin-on HMDS 3krpm 30", prior to NR9-6000PY |
||
|- |
|||
| colspan="10" |*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal |
|||
<nowiki>**</nowiki> To use AZ5214 as a negative PR requires Flood Exposure with the [[Contact Aligner (SUSS MA-6)|MA6]] or [[Suss Aligners (SUSS MJB-3)|MJB]] aligner '''''after PEB''''', before developing. See here for a [[AZ5214 - Basic Process|basic AZ5214 process]], it is different than typical negative resists. |
|||
|} |
|} |
||
=== SU-8 Recipes === |
|||
Staff-developed recipes for SU-8: |
|||
*[//wiki.nanotech.ucsb.edu/w/images/1/1e/47-Photolithography_of_SU8-2005.pdf SU-8-2005 Recipe] |
*[//wiki.nanotech.ucsb.edu/w/images/1/1e/47-Photolithography_of_SU8-2005.pdf SU-8-2005 Recipe] |
Latest revision as of 23:41, 22 August 2024
Back to Lithography Recipes.
Notes
Below is a listing of contact lithography recipes for use with designated aligners.
Based on your sample reflectivity, absorption, and surface topography the exposure time parameters may vary. This listing is a guideline to get you started.
For best resolution using thin resists, you will need to remove any edge bead before contact and exposure. This can be done with a razor blade (not for brittle substrates), or EBR-100 on a cotton swab (wipe off excess liquid before using), or lithgraphically with a tin-foil mask, flood exposure and develop.
Also, hard contact mode will give you the most intimate contact between sample and mask, giving the best resolution. However for flat unpatterned substrates, this can cause wafers to stick to the mask plate.
Post develop bakes (not listed, aka. "hard bake") are used to make the resist more etch resistant and depend on subsequent processes. Unless otherwise noted, all exposures are done on silicon wafers.
Suss Aligners (SUSS MJB-3)
Positive Resist (MJB-3)
Unless otherwise noted, bakes are on hot plates and the exposure of the resist is done using no filtering at 7.0 mW/cm2. Only Channel @2 is used/calibrated. Power of the lamp is set using the 405 nm (h-line) detector.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|
AZ4110 | 4 krpm/30” | 95°C/60” | ~ 1.1 um | 8” | AZ400K:DI 1:4 | 50" | |
AZ4210 | 4 krpm/30” | 95°C/60” | ~ 2.1 um | 13” | AZ400K:DI 1:4 | 70” | |
AZ4330 | 4 krpm/30” | 95°C/60” | ~ 3.3 um | 18” | AZ400K:DI 1:4 | 90” | |
SPR220-3.0 | 3.5 krpm/30” | 115°C/90” | ~ 2.5 um | 25” | AZ300MIF | 50” |
|
SPR220-7.0 | 3.5 krpm/45” | 115°C/120” | ~ 7.5 um | 60” | AZ300MIF | 70” |
Negative Resist (MJB-3)
Unless otherwise noted, bakes are on hot plates and the exposure of the resist is done using no filtering at 7.0 mW/cm2. Power of the lamp is set using the 405 nm (h-line) detector. In general, many negative resists require post-exposure-bakes (PEB) / flood exposures in order to make the negative tone of the image. All flood exposures are done in broadband light using any contact aligner. Also, because the tone is negative, a shorter first exposure time will result in more undercut, which is desirable for single-layer lift-off processes. Under these conditions more develop time will also give more undercut.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | PEB* | Flood** | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|
AZ5214** | 6 krpm/30” | 95°C/60” | ~ 1 um | 5” | 110°C/60” | 60” | AZ400K:DI 1:5.5 or AZ300MIF |
60" 45" |
|
AZ5214** | 6 krpm/30” | 95°C/60” | ~ 1 um | 10” | 110°C/60” | 60” | AZ300MIF | 45” |
|
AZnLOF2020 | 3 krpm/30” | 110°C/90” | ~ 2.1 um | 10” | 110°C/60” | AZ300MIF | 60” |
| |
NR9-6000PY | 3 krpm/30” | 140°C/180” | ~ um | 30” | 100°C/60” | AZ300MIF | 30” |
| |
*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal
** To use AZ5214 as a negative PR requires Flood Exposure with the MA6 or MJB aligner after PEB, before developing. See here for a basic AZ5214 process, it is different than typical negative resists. |
Contact Aligner (SUSS MA-6)
Positive Resist (MA-6)
Unless otherwise noted, bakes are on hot plates and the exposure of the resist is done using no filtering at 9 mW/cm2 (Channel 1). Power of the lamp is set using the 365 nm (i-line) detector. For reference, this would equate to 17.5 mW/cm² when measured with a 405 nm (h-line) detector.
For the MA-6 aligner, using Channel 1, the exposure times given below are the same as the MJB-3 except they have been reduced by a factor of 2.4.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|
AZ4110 | 4 krpm/30” | 95°C/60” | ~ 1.1 um | 3.3” | AZ400K:DI 1:4 | 50" | |
AZ4210 | 4 krpm/30” | 95°C/60” | ~ 2.1 um | 5.4” | AZ400K:DI 1:4 | 70” | |
AZ4330 | 4 krpm/30” | 95°C/60” | ~ 3.3 um | 7.5” | AZ400K:DI 1:4 | 90” | |
SPR955CM-0.9 | 3 krpm/30” | 95°C/60” | ~ 0.9 um | 8” | AZ300MIF | 70” |
|
SPR220-3.0 | 3.5 krpm/30” | 115°C/90” | ~ 2.5 um | 10.4” | AZ300MIF | 50” |
|
SPR220-7.0 | 3.5 krpm/45” | 115°C/120” | ~ 7.5 um | 25” | AZ300MIF | 70” |
Negative Resist (MA-6)
Unless otherwise noted, bakes are on hot plates and the exposure of the resist is done using no filtering at 9 mW/cm2 (Channel 1). Power of the lamp is set using the 365 nm (i-line) detector. For reference, this would equate to 17.5 mW/cm² when measured with a 405 nm (h-line) detector.
In general, many negative resists require post-exposure-bakes (PEB) / flood exposures in order to make the negative tone of the image. All flood exposures are done in broadband light using any contact aligner. Also, because the tone is negative, a shorter first exposure time will result in more undercut, which is desirable for single-layer lift-off processes. Under these conditions more develop time will also give more undercut. For the MA-6 aligner, using Channel 1, the exposure times given below are the same as the MJB-3 except they have been reduced by a factor of 2.4.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | PEB* | Flood Exposure** | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|
AZ5214** | 6 krpm/30” | 95°C/60” | ~ 1 um | 2.1” | 110°C/60” | 30" | AZ400K:DI 1:5.5 or AZ300MIF |
60" 45" |
|
AZnLOF2020 | 3 krpm/30” | 110°C/90” | ~ 2.1 um | 4.2” | 110°C/60” | AZ300MIF | 60” |
| |
AZnLOF2035 | 2.5 krpm/30” | 110°C/60” | ~ 3.5 um | 5.0” | 110°C/60” | AZ300MIF | 70” |
| |
NR9-6000PY | 3 krpm/30” | 140°C/180” | ~ um | 13.1” | 100°C/60” | AZ300MIF | 30” |
| |
*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal
** To use AZ5214 as a negative PR requires Flood Exposure with the MA6 or MJB aligner after PEB, before developing. See here for a basic AZ5214 process, it is different than typical negative resists. |
SU-8 Recipes
Staff-developed recipes for SU-8: