Vacuum Deposition Recipes: Difference between revisions
Jump to navigation
Jump to search
(added Thermal Evap rankings to wiki) |
(Added AuSn to Thermal evap 2) |
||
(2 intermediate revisions by the same user not shown) | |||
Line 60: | Line 60: | ||
| |
| |
||
| |
| |
||
| |
|||
⚫ | |||
| |
| |
||
| |
| |
||
Line 77: | Line 77: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 128: | Line 128: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 163: | Line 163: | ||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
||
| |
| |
||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!AuSn |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
⚫ | |||
| |
| |
||
| |
| |
||
Line 230: | Line 247: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 247: | Line 264: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 264: | Line 281: | ||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
Line 281: | Line 298: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 298: | Line 315: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 315: | Line 332: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 434: | Line 451: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 451: | Line 468: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 468: | Line 485: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 553: | Line 570: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 587: | Line 604: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 603: | Line 620: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 638: | Line 655: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 655: | Line 672: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 706: | Line 723: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 722: | Line 739: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R2]] |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 740: | Line 757: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 756: | Line 773: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 774: | Line 791: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 791: | Line 808: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 807: | Line 824: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
|<br> |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 825: | Line 842: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 841: | Line 858: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
|<br> |
|||
| |
|||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 910: | Line 927: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 927: | Line 944: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 961: | Line 978: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 995: | Line 1,012: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 1,012: | Line 1,029: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 1,029: | Line 1,046: | ||
| bgcolor="#eeffff" |R1 |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R3] |
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R3] |
||
Line 1,080: | Line 1,097: | ||
| bgcolor="#eeffff" |[[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R6]] |
| bgcolor="#eeffff" |[[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R6]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R6]] |
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R6]] |
||
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]] |
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]] |
||
Line 1,182: | Line 1,199: | ||
| bgcolor="#eeffff" |R1 |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 1,199: | Line 1,216: | ||
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]] |
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]] |
||
|<br> |
|<br> |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 1,216: | Line 1,233: | ||
| bgcolor="#eeffff" |R1 |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 1,267: | Line 1,284: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 1,284: | Line 1,301: | ||
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]] |
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 1,301: | Line 1,318: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 1,318: | Line 1,335: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 1,335: | Line 1,352: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 1,368: | Line 1,385: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 1,386: | Line 1,403: | ||
| |
| |
||
| |
| |
||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 1,420: | Line 1,437: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
Revision as of 21:57, 7 November 2024
Process Control Data
See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.
Deposition Tools/Materials Table
The Key/Legend for this table's A...R6
values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
Process Level | Description of Process Level Ranking | ||||||||||
A | Process Allowed and materials available but never done | ||||||||||
R1 | Process has been ran at least once | ||||||||||
R2 | Process has been ran and/or procedure is documented or/and data available | ||||||||||
R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
R4 | Process has a documented procedure with regular (≥4x per year) data or lookahead/in-Situ control available | ||||||||||
R5 | Process has a documented procedure with regular (≥4x per year) data and lookahead/in-Situ control available | ||||||||||
R6 | Process has a documented procedure, regular ( ≥4x per year) data, and control charts/limits available |