=[[Atomic Layer Deposition (Oxford FlexAL)]]= |
=[[Atomic Layer Deposition (Oxford FlexAL)]]= |
||
== |
==Oxford FlexAL Process Notes== |
||
===Temperature=== |
|||
"Thermal" ALD, considered the most standard process. Can be slower due to time for reaction to proceed. |
|||
''To Be Added: effect of varying temeprature'' |
|||
===Plasma=== |
|||
'''''O*''''' or '''''N*''''' mean Oxygen/Nitrogen plasma, respectively. |
|||
The plasma processes on this tool will run considerably faster than purely thermal proceses, because the reaction time is faster. Also, the O* plasma may reduce carbon contaminants from the organic precursors. |
|||
The drawback is that the plasma shutter, which opens/closes between plasma steps, gets coated in materials and can cause higher particle counts. We have attempted to remedy this by keeping the plasma shutter open during all recipes. |
|||
===Ozone=== |
|||
'''''O3''''' indicates a recipe using the Ozone generator for reaction. This Ozone-generator must be manually turned on before running the recipe - check with [[Atomic Layer Deposition (Oxford FlexAL)|supervisor]] for details. |
|||
''More info to be added'' |
|||
===Varying Atomic Ratios=== |
|||
For some recipes such as TiN, there are two loops in the recipe. The outermost loop controls the total thickness of the film, the inner loop controls the ratio between the two elements. Contact the superviosr for more detailed info. |
|||
==Oxford FlexAL Chamber #1: Metals== |
|||
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.) |
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.) |
||
''Note that Plasma-based (indicated by asterisk eg.'' N* ''or'' O*'') recipes run nearly 2x faster than H2O/thermal recipes due to faster reaction rate, thus shorter cycling.'' |
|||
=== |
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 1)=== |
||
⚫ | |||
⚫ | |||
**This is considered the standard recipe for ALD |
|||
⚫ | |||
**Recipe variations: ''TBD'' |
|||
===Pt deposition (ALD CHAMBER 1)=== |
|||
*Recipe name: '''''Ch1_TMCpPt+O3-300C''''' |
*Recipe name: '''''Ch1_TMCpPt+O3-300C''''' |
||
**Pt deposition rate ~ 0.5-0.6 A/cyc |
**Pt deposition rate ~ 0.5-0.6 A/cyc |
||
Line 18: | Line 48: | ||
**300°C deposition |
**300°C deposition |
||
=== |
===Ru deposition (ALD CHAMBER 1)=== |
||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
===SiO{{sub|2}} deposition (ALD CHAMBER 1)=== |
|||
⚫ | |||
⚫ | |||
**Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp. |
|||
⚫ | |||
⚫ | |||
**SiO<sub>2</sub> deposition rate ~ 1.008 A/cyc |
|||
**Similar to above TDMAS recipes, with different precursor gas. |
|||
⚫ | |||
**Etch rate (BHF:DI=1:100)~7.46nm/min |
|||
⚫ | |||
''Conductive film.'' |
''Conductive film.'' |
||
* |
*Recipe name: '''''Ch1_DEZ+H2O-200C''''' |
||
⚫ | |||
*ZnO deposition rate ≈ 1.6 A/cycle |
|||
*resistivity ≈ ''TBA'' |
*resistivity ≈ ''TBA'' |
||
*200°C Deposition, Water reaction |
*200°C Deposition, Water reaction |
||
=== |
===ZnO:Al deposition (ALD CHAMBER 1)=== |
||
''Al-Doped ZnO for variable resisitivity.'' |
''Al-Doped ZnO for variable resisitivity.'' |
||
*Recipe name: '''''Ch1_DEZ/TMA+H2O-200C''''' |
*Recipe name: '''''Ch1_DEZ/TMA+H2O-200C''''' |
||
**''The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.'' |
**''The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.'' |
||
*Al dose fraction = 5% for lowest resistivity |
*Al dose fraction = 5% for lowest resistivity |
||
*ZnO deposition rate ~ 1.7A/cyc |
*ZnO deposition rate ~ 1.7A/cyc |
||
*resistivity ~ 4200uOhm.cm (390A film) |
*resistivity ~ 4200uOhm.cm (390A film) |
||
== |
==Oxford FlexAL Chamber #3: Dielectrics== |
||
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.) |
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.) |
||
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)=== |
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''CH3-TMA+H2O-<u>300C</u>''''' |
*Recipe name: '''''CH3-TMA+H2O-<u>300C</u>''''' ("Thermal") |
||
**300°C Dep., Thermal Water reaction |
|||
⚫ | |||
⚫ | |||
**This is considered the standard recipe for ALD |
**This is considered the standard recipe for ALD |
||
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1.192 A/cyc |
|||
⚫ | |||
*Recipe |
*Recipe name: '''''CH3-TMA+H2O-25<u>0C</u>''''' ("Thermal") |
||
** |
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1.214 A/cyc |
||
**Temperature variations: 300°C (std.), '''250°C, 200°C, 150°C, 120°C''' |
|||
⚫ | |||
**Oxygen Plasma reaction instead of H2O |
**Oxygen Plasma reaction instead of H2O |
||
**Lower carbon content |
**Lower carbon content |
||
**Approx. <u>1.5–2x faster deposition rate</u> than thermal. |
|||
⚫ | |||
**Temperature variations: 300°C (std.), '''200°C, 120°C''' |
|||
⚫ | |||
⚫ | |||
**Similar dep. rate |
**Similar dep. rate |
||
**Ozone (O<sub>3</sub>) reactant, experimental |
**Ozone (O<sub>3</sub>) reactant, experimental |
||
**Requires Ozone generator to be turned on - ask supervisor |
|||
===AlN deposition (ALD CHAMBER 3)=== |
===AlN deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''CH3-TMA+100W/N*-300C''''' |
*Recipe name: '''''CH3-TMA+100W/N*-300C''''' |
||
**AlN deposition rate ~ t.b.d. |
**AlN deposition rate ~ t.b.d. |
||
Line 67: | Line 116: | ||
===HfO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===HfO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
⚫ | |||
*Recipe name: '''''CH3-TEMAH+H2O-300C''''' ("Thermal") |
|||
**HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
**HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
||
**Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
**Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
||
**Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C |
**Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C |
||
*Recipe name: '''''CH3-TEMAH+250W/O*-300C''''' |
*Recipe name: '''''CH3-TEMAH+250W/O*-300C''''' ("Plasma") |
||
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
||
*Recipe name: '''''CH3-TEMAH+O3/100mT-300C''''' |
*Recipe name: '''''CH3-TEMAH+O3/100mT-300C''''' ("Ozone") |
||
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
||
**Requires Ozone generator to be turned on - ask supervisor |
|||
===SiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===SiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
⚫ | |||
*Recipe name: '''''CH3-TDMAS+250W/O*-<u>300C</u>''''' ("Plasma") |
|||
**SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc |
**SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc |
||
**Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp. |
**Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp. |
||
**Temperature variations: 300 |
**Temperature variations: <u>300°C</u> (std.), 250°C, 230°C, 220°C, 200°C, 175°C, 150°C, 120°C |
||
*Recipe name: '''''CH3-TDMAS+O3/200mT-300C''''' |
*Recipe name: '''''CH3-TDMAS+O3/200mT-300C''''' ("Ozone") |
||
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
||
**Requires Ozone generator to be turned on - ask supervisor |
|||
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
⚫ | |||
*Recipe name: '''''CH3-TEMAZ+H2O-<u>300C</u>''''' ("Thermal") |
|||
**ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
**ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
||
**Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above. |
**Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above. |
||
**Temperature variations: 300°C (std.), 200°C |
**Temperature variations: <u>300°C</u> (std.), 200°C |
||
*Recipe name: '''''CH3-TEMAZ+250W/O*-300C''''' |
*Recipe name: '''''CH3-TEMAZ+250W/O*-300C''''' ("Plasma") |
||
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
||
*Recipe name: '''''CH3-TEMAZ+O3/100mT-300C''''' |
*Recipe name: '''''CH3-TEMAZ+O3/100mT-300C''''' ("Ozone") |
||
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
||
**Requires Ozone generator to be turned on - ask supervisor |
|||
===TiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===TiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
⚫ | |||
*Recipe name: '''''CH3-TDMAT+H2O-300C''''' ("Thermal") |
|||
**TiO<sub>2</sub> deposition rate ~ 0.6A/cyc |
**TiO<sub>2</sub> deposition rate ~ 0.6A/cyc |
||
**Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
**Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
||
**Temperature variations: 300°C (std.), 200°C, 120*C |
**Temperature variations: 300°C (std.), 200°C, 120*C |
||
*Recipe name: '''''CH3-TDMAT+250W/O*-300C''''' |
*Recipe name: '''''CH3-TDMAT+250W/O*-300C''''' ("Plasma") |
||
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
||
===TiN deposition (ALD CHAMBER 3)=== |
===TiN deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''CH3-TDMAT+400W/12N*/4H*-300C''''' |
*Recipe name: '''''CH3-TDMAT+400W/12N*/4H*-300C''''' |
||
**TiN deposition rate ~ 0.7A/cyc |
**TiN deposition rate ~ 0.7A/cyc |
||
Line 114: | Line 171: | ||
**Uses Plasma of NH<sub>3</sub> only |
**Uses Plasma of NH<sub>3</sub> only |
||
**Temperatures: 300°C (std.), 200°C |
**Temperatures: 300°C (std.), 200°C |
||
===Historical Data (ALD Chamber 3)=== |
|||
*[[Tbd|2021 ALD Al2O3 (H2O, 300°C) Historical Data]] |
Latest revision as of 00:42, 15 November 2024
Back to Vacuum Deposition Recipes.
Atomic Layer Deposition (Oxford FlexAL)
Oxford FlexAL Process Notes
Temperature
"Thermal" ALD, considered the most standard process. Can be slower due to time for reaction to proceed.
To Be Added: effect of varying temeprature
Plasma
O* or N* mean Oxygen/Nitrogen plasma, respectively.
The plasma processes on this tool will run considerably faster than purely thermal proceses, because the reaction time is faster. Also, the O* plasma may reduce carbon contaminants from the organic precursors.
The drawback is that the plasma shutter, which opens/closes between plasma steps, gets coated in materials and can cause higher particle counts. We have attempted to remedy this by keeping the plasma shutter open during all recipes.
Ozone
O3 indicates a recipe using the Ozone generator for reaction. This Ozone-generator must be manually turned on before running the recipe - check with supervisor for details.
More info to be added
Varying Atomic Ratios
For some recipes such as TiN, there are two loops in the recipe. The outermost loop controls the total thickness of the film, the inner loop controls the ratio between the two elements. Contact the superviosr for more detailed info.
Oxford FlexAL Chamber #1: Metals
Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)
Al2O3 deposition (ALD CHAMBER 1)
- Recipe name: CH3-TMA+H2O-300C ("Thermal")
- 300°C Dep., Thermal Water reaction
- This is considered the standard recipe for ALD
- Al2O3 deposition rate ~ 1.265 A/cyc
- Recipe variations: TBD
Pt deposition (ALD CHAMBER 1)
- Recipe name: Ch1_TMCpPt+O3-300C
- Pt deposition rate ~ 0.5-0.6 A/cyc
- Conductivity data: (to be added)
- recipe utilizes the ozone generator which must be first set to the following conditions:
- O2 flow = 250sccm
- O3 concentration = 15 wt%
- 300°C deposition
- Recipe name: CH1-TMCpPt+250W/O*-300C
- Uses Oxygen plasma
- 300°C deposition
Ru deposition (ALD CHAMBER 1)
- Recipe name: Ch1_Ex03Ru[HPbub]+O2-300C
- Ru deposition rate ~ 0.6-0.7A/cyc.
- Conductivity data: (to be added)
- 300°C, O2 gas reaction
SiO2 deposition (ALD CHAMBER 1)
- Recipe name: CH3-TDMAS+250W/O*-300C ("Plasma")
- SiO2 deposition rate ~ 0.7-0.8A/cyc
- Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
- Temperature variations: 300*C (std.), 250°C, 200°C, 120°C
- Recipe name: CH1-BDEAS-O*/300W-300C
- SiO2 deposition rate ~ 1.008 A/cyc
- Similar to above TDMAS recipes, with different precursor gas.
- Temperature variations: To Be Added
- Etch rate (BHF:DI=1:100)~7.46nm/min
ZnO Deposition (ALD Chamber 1)
Conductive film.
- Recipe name: Ch1_DEZ+H2O-200C
- ZnO deposition rate ≈ 1.6 A/cycle
- resistivity ≈ TBA
- 200°C Deposition, Water reaction
ZnO:Al deposition (ALD CHAMBER 1)
Al-Doped ZnO for variable resisitivity.
- Recipe name: Ch1_DEZ/TMA+H2O-200C
- The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.
- Al dose fraction = 5% for lowest resistivity
- ZnO deposition rate ~ 1.7A/cyc
- resistivity ~ 4200uOhm.cm (390A film)
Oxford FlexAL Chamber #3: Dielectrics
Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)
Al2O3 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TMA+H2O-300C ("Thermal")
- 300°C Dep., Thermal Water reaction
- This is considered the standard recipe for ALD
- Al2O3 deposition rate ~ 1.192 A/cyc
- Recipe name: CH3-TMA+H2O-250C ("Thermal")
- Al2O3 deposition rate ~ 1.214 A/cyc
- Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
- Recipe Name: CH3-TMA+250W/O*-300C ("Plasma")
- Oxygen Plasma reaction instead of H2O
- Lower carbon content
- Approx. 1.5–2x faster deposition rate than thermal.
- Temperature variations: 300°C (std.), 200°C, 120°C
- Recipe Name: CH3-TMA+O3/200mT-300C ("Ozone")
- Similar dep. rate
- Ozone (O3) reactant, experimental
- Requires Ozone generator to be turned on - ask supervisor
AlN deposition (ALD CHAMBER 3)
- Recipe name: CH3-TMA+100W/N*-300C
- AlN deposition rate ~ t.b.d.
- Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
- Temperature Variations: 300°C Dep. (std.), 200*C, 120°C
- Power variations: 300W, 400W (at 300°C)
- Nitrogen/Hydrogen variations: "30N*/30H*" at 200*C and 300°C
HfO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TEMAH+H2O-300C ("Thermal")
- HfO2 deposition rate ~ 0.9-1.0A/cyc
- Note: deposition shows significant parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
- Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
- Recipe name: CH3-TEMAH+250W/O*-300C ("Plasma")
- Uses Oxygen plasma reactant instead of H2O
- Recipe name: CH3-TEMAH+O3/100mT-300C ("Ozone")
- Uses Ozone (O3) for reactant instead of H2O
- Requires Ozone generator to be turned on - ask supervisor
SiO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TDMAS+250W/O*-300C ("Plasma")
- SiO2 deposition rate ~ 0.7-0.8A/cyc
- Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
- Temperature variations: 300°C (std.), 250°C, 230°C, 220°C, 200°C, 175°C, 150°C, 120°C
- Recipe name: CH3-TDMAS+O3/200mT-300C ("Ozone")
- Uses Ozone (O3) for reactant instead of H2O
- Requires Ozone generator to be turned on - ask supervisor
ZrO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TEMAZ+H2O-300C ("Thermal")
- ZrO2 deposition rate ~ 0.9-1.0A/cyc
- Not directly characterized since results are basically the same as the HfO2 process above.
- Temperature variations: 300°C (std.), 200°C
- Recipe name: CH3-TEMAZ+250W/O*-300C ("Plasma")
- Uses Oxygen plasma reactant instead of H2O
- Recipe name: CH3-TEMAZ+O3/100mT-300C ("Ozone")
- Uses Ozone (O3) for reactant instead of H2O
- Requires Ozone generator to be turned on - ask supervisor
TiO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TDMAT+H2O-300C ("Thermal")
- TiO2 deposition rate ~ 0.6A/cyc
- Note: deposition shows parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
- Temperature variations: 300°C (std.), 200°C, 120*C
- Recipe name: CH3-TDMAT+250W/O*-300C ("Plasma")
- Uses Oxygen plasma reactant instead of H2O
TiN deposition (ALD CHAMBER 3)
- Recipe name: CH3-TDMAT+400W/12N*/4H*-300C
- TiN deposition rate ~ 0.7A/cyc
- Conductivity data: (to be added)
- Uses Plasma of N2 & H2 gases.
- Temperatures: 300°C (std.), 200°C
- Recipe name: CH3-TDMAT+100W/N*-300C
- Uses Plasma of N2 only
- Temperatures: 300°C (std.), 200°C
- Recipe name: CH3-TDMAT+100W/NH3*-300C
- Uses Plasma of NH3 only
- Temperatures: 300°C (std.), 200°C