Vacuum Deposition Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
No edit summary |
|||
| (49 intermediate revisions by 6 users not shown) | |||
| Line 1: | Line 1: | ||
===[[Process Group - Process Control Data#Deposition .28Process Control Data.29|<u>Process Control Data</u>]]=== |
|||
{{Recipe Table Explanation}} |
|||
<small>''See [[Process Group - Process Control Data#Deposition .28Process Control Data.29|linked page]] for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.''</small> |
|||
===Deposition Tools/Materials Table=== |
|||
''The Key/Legend for this table's <code>R1...R6</code> values is at the [[Vacuum Deposition Recipes#Process Ranking Table|<u>bottom of the page</u>]].'' |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
! colspan=" |
! colspan="16" width="1675" height="45" |<div style="font-size: 150%;">Vacuum Deposition Recipes</div> |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
| |
|<!-- INTENTIONALLY LEFT BLANK --><br> |
||
! colspan="4" bgcolor="#d0e7ff" align="center" | |
! colspan="4" bgcolor="#d0e7ff" align="center" |'''[[E-Beam Evaporation Recipes|E-Beam Evaporation]]''' |
||
! colspan=" |
! colspan="4" |'''[[Sputtering Recipes|Sputtering]]''' |
||
! colspan="2" bgcolor="#d0e7ff" align="center" | |
! colspan="2" bgcolor="#d0e7ff" align="center" |'''[[Thermal Evaporation Recipes|Thermal Evaporation]]''' |
||
! colspan="3" bgcolor="#d0e7ff" align="center" | |
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[PECVD Recipes|Plasma Enhanced Chemical<br>Vapor Deposition (PECVD)]]''' |
||
! width="90" bgcolor="#d0e7ff" align="center" | |
! width="90" bgcolor="#d0e7ff" align="center" |'''[[Atomic Layer Deposition Recipes|Atomic Layer Deposition]]''' |
||
! width="80" bgcolor="#d0e7ff" align="center" | |
! width="80" bgcolor="#d0e7ff" align="center" |'''[[Molecular Vapor Deposition Recipes|Molecular Vapor Deposition]]''' |
||
|- |
|- |
||
! width="20" bgcolor="#d0e7ff" align="center" | |
! width="20" bgcolor="#d0e7ff" align="center" |'''Material''' |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_3_.28Temescal.29|E-Beam 3 (Temescal)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_4_.28CHA.29|E-Beam 4 (CHA)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29|Sputter 3<br>(AJA ATC 2000-F)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(AJA ATC 2200-V)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_5_.28AJA_ATC_2200-V.29 Sputter 5 (AJA ATC 2200-V)] |
||
| width=" |
| width="55" bgcolor="#daf1ff" |[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]] |
||
| width=" |
| width="45" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]] |
||
| width=" |
| width="65" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_2_.28Solder.29|Thermal Evap 2 (Solder)]] |
||
| width=" |
| width="65" bgcolor="#daf1ff" |[[PECVD Recipes#PECVD_1_.28PlasmaTherm_790.29|PECVD 1<br>(PlasmaTherm 790)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[PECVD Recipes#PECVD_2_.28Advanced_Vacuum.29|PECVD 2<br>(Advanced Vacuum)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29|Unaxis VLR ICP-PECVD]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[Atomic_Layer_Deposition_Recipes|Atomic Layer Deposition (Oxford FlexAL)]] |
||
| width="65" bgcolor="#daf1ff" | |
| width="65" bgcolor="#daf1ff" |[[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]] |
||
| width="65" bgcolor="#daf1ff" | [[Atomic_Layer_Deposition_Recipes|Atomic Layer Deposition (Oxford FlexAL)]] |
|||
| width="65" bgcolor="#daf1ff" | [[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]] |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Ag |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!AgBr |
|||
! bgcolor="#d0e7ff" align="center" | Al |
|||
| |
|||
| {{Al/E1}} |
|||
| |
|||
| <br> |
|||
| |
|||
| {{Al/E3}} |
|||
| |
|||
| {{Al/E4}} |
|||
| |
|||
| <br> |
|||
| |
|||
| {{rl|Sputtering Recipes|Al deposition (Sputter 2)}} |
|||
| |
|||
| [[Sputtering Recipes|A]] |
|||
| |
|||
| {{rl|Sputtering Recipes|Al Deposition (Sputter 4)}} |
|||
| |
|||
| <br> |
|||
| |
|||
| <br>[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]] |
|||
| |
|||
| [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
!AgCl |
|||
! bgcolor="#d0e7ff" align="center" | Al<sub>2</sub>O<sub>3</sub> |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E2}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|Al2O3 Deposition (Sputter 4)}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [https://www.nanotech.ucsb.edu/wiki/index.php/Sputtering_Recipes#Al2O3_deposition_.28IBD.29 R] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | {{rl|Atomic Layer Deposition Recipes|Al2O3 deposition (ALD)}} |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Al |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| <br> |
|||
| |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| <br> |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| <br> |
|||
|[[Sputtering Recipes|R1]] |
|||
| <br> |
|||
| |
|[[Sputtering Recipes|R3]] |
||
| |
|[[Sputtering Recipes|R1]] |
||
|R1 |
|||
| [[Sputtering Recipes|A]] |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
| <br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| [[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]] |
|||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| {{rl|Atomic Layer Deposition Recipes|AlN deposition (ALD)}} |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|R4]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!As |
|||
! bgcolor="#d0e7ff" align="center" | B |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
!AuPd |
|||
! bgcolor="#d0e7ff" align="center" | C |
|||
| |
|||
| bgcolor="#eeffff" align="center" | {{rl|E-Beam Evaporation Recipes|Materials Table (E-Beam #1)}} |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| |
|||
| bgcolor="#eeffff" align="center" | |
|||
| bgcolor="#eeffff" align="center" | |
|||
| bgcolor="#eeffff" align="center" | |
|||
|- |
|- |
||
!AuZn |
|||
! bgcolor="#d0e7ff" align="center" | CeO<sub>2</sub> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|E-Beam Evaporation Recipes|E-Beam 2 (Custom)|CeO<sub>2</sub> deposition (E-Beam 2)}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!AuSn |
|||
! bgcolor="#d0e7ff" align="center" | Co |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E4}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|R]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!AuGe |
|||
! bgcolor="#d0e7ff" align="center" | Cr |
|||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
| {{Al/E1}} |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| {{Al/E4}} |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Sputtering Recipes|R]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |AlN |
||
|<br> |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}} |
|||
|R1 |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R4]] |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Au |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| {{Al/E1}} |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| <br> |
|||
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Au|R6]] |
|||
| {{Al/E4}} |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| <br> |
|||
| bgcolor="#eeffff" |R3 |
|||
| <br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| [[Sputtering Recipes|R]] |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
| <br> |
|||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
|||
| <br> |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |B |
||
|<br> |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | {{Al/E3}} |
|||
|<br> |
|||
| bgcolor="#eeffff" | {{Al/E4}} |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
|<br> |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!Be |
|||
! bgcolor="#d0e7ff" align="center" | GeO<sub>2</sub> |
|||
| |
| |
||
| |
|||
| {{Al/E2}} |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |C |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R3]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!Cd |
|||
! bgcolor="#d0e7ff" align="center" | Hf |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!CdS |
|||
! bgcolor="#d0e7ff" align="center" | HfO<sub>2</sub> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Sputtering Recipes|A]] |
|||
| |
|||
| [[Sputtering Recipes|A]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| {{rl|Atomic Layer Deposition Recipes|HfO2 deposition (ALD)}} |
|||
| <br> |
|||
|- |
|- |
||
!CdTe |
|||
! bgcolor="#d0e7ff" align="center" | In |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!CaF2 |
|||
! bgcolor="#d0e7ff" align="center" | Ir |
|||
| |
|||
| {{Al/E1}} |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |CeO<sub>2</sub> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R3]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Co |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| [[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| [[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| |
|||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Cr |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
| |
|||
|<br> |
|||
| {{Al/E2}} |
|||
|<br> |
|||
| |
|||
|[[Process Group - Process Control Data#E-Beam 4: Cr|R6]] |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R3] |
|||
| |
|||
|<br> |
|||
| |
|||
|{{Rl|Sputtering_Recipes|Sputter_5_.28AJA_ATC_2200-V.29|R3}} |
|||
| |
|||
|<br> |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
|||
| |
|||
|<br> |
|||
| |
|||
|<br> |
|||
| |
|||
|<br> |
|||
| |
|||
|<br> |
|||
| |
|||
|<br> |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Cu |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Fe |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| {{Al/E1}} |
|||
| |
|<br> |
||
| |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| <br> |
|||
|[[Sputtering Recipes|R3]] |
|||
| <br> |
|||
| |
|<br> |
||
| |
|<br> |
||
|<br> |
|||
| [[Sputtering Recipes|R]] |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| <br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| <br> |
|||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
!Ga |
|||
! bgcolor="#d0e7ff" align="center" | Nd |
|||
| |
| |
||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Sputtering Recipes|A]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
!GaAs |
|||
! bgcolor="#d0e7ff" align="center" | Ni |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E3}} |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E4}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Ge |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| {{Al/E1}} |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| {{Al/E4}} |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| bgcolor="#eeffff" |<br> |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |GeO<sub>2</sub> |
||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E4}} |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Gd |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| {{Al/E1}} |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
|||
| {{Al/E3}} |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
|||
| {{Al/E4}} |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
|||
| [[Thermal Evaporation Recipes|A]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| [[Thermal Evaporation Recipes|A]] |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Hf |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br>[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | {{rl|Atomic Layer Deposition Recipes|Pt deposition (ALD)}} |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub> |
||
|<br> |
|||
| {{Al/E1}} |
|||
| |
|<br> |
||
| |
|<br> |
||
|<br> |
|||
| {{Al/E4}} |
|||
|[[Sputtering Recipes|R1]] |
|||
| <br> |
|||
|[[Sputtering Recipes|R1]] |
|||
| <br> |
|||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R4]] |
|||
| <br> |
|||
| |
|<br> |
||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
!Hg |
|||
! bgcolor="#d0e7ff" align="center" | Si |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E2}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|R]] |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br>[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|PECVD Recipes|PECVD 2 (Advanced Vacuum)|Amorphous-Si deposition (PECVD#2|Amorphous Si Films and Their Stress}} |
|||
| |
|||
| bgcolor="#eeffff" | [[PECVD_Recipes#Amorphous_Si_.28100.25SiH4_Ar_He.29|R]] |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |In |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
|||
| {{rl|Sputtering Recipes|SiN deposition (Sputter 3)}} |
|||
| bgcolor="#eeffff" |<br> |
|||
| [[Sputtering Recipes|A]] |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R3]] |
|||
| [[Sputtering_Recipes#Si3N4_deposition_.28IBD.29|R]] |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
|||
| {{rl|PECVD Recipes|SiN deposition (PECVD #1)}} |
|||
| bgcolor="#eeffff" |<br> |
|||
| {{rl|PECVD Recipes|SiN deposition (PECVD #2)}} |
|||
| bgcolor="#eeffff" |<br> |
|||
| {{rl|PECVD Recipes|SiN deposition (Unaxis VLR)}} |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
!InSb |
|||
! bgcolor="#d0e7ff" align="center" | SiO<sub>2</sub> |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E2}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|SiO2 deposition (Sputter 3)}} |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|PECVD Recipes|SiO2 deposition (PECVD #1)}} |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|PECVD Recipes|SiO2 deposition (PECVD #2)}} |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|PECVD Recipes|SiO2 deposition (Unaxis VLR)}} |
|||
| bgcolor="#eeffff" | {{rl|Atomic Layer Deposition Recipes|SiO2 deposition (ALD)}} |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Ir |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
| <br> |
|||
| |
|<br> |
||
| |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
|||
| <br> |
|||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|<br> |
||
| |
|||
| <br> |
|||
| |
|||
| [https://www.nanotech.ucsb.edu/wiki/index.php/Sputtering_Recipes#SiOxNy_deposition_.28IBD.29 A] |
|||
| |
|<br> |
||
| |
|<br> |
||
|<br> |
|||
| [[PECVD_Recipes#PECVD_1_.28PlasmaTherm_790.29|R]] |
|||
| |
|<br> |
||
| |
|<br> |
||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |ITO |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R3]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!KCl |
|||
! bgcolor="#d0e7ff" align="center" | SrF<sub>2</sub> |
|||
| |
|||
| <br> |
|||
| |
|||
| {{Al/E2}} |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
!LiF |
|||
! bgcolor="#d0e7ff" align="center" | Ta |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|Ta deposition (Sputter 3)}} |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br>[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!Mg |
|||
! bgcolor="#d0e7ff" align="center" | Ta<sub>2</sub>O<sub>5</sub> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| {{Al/E2}} |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| <br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| [[Sputtering_Recipes#Ta2O5_deposition_.28IBD.29|R]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |MgF2 |
||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E3}} |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E4}} |
|||
|[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}} |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|Ti-Au Deposition (Sputter 4)}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| bgcolor="#eeffff" | <br>[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |MgO |
||
| |
|||
| <br> |
|||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Sputtering Recipes|A]] |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Sputtering Recipes|R]] |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| {{rl|Atomic Layer Deposition Recipes|TiN deposition (ALD)}} |
|||
| <br> |
|||
|- |
|- |
||
!Mn |
|||
! bgcolor="#d0e7ff" align="center" | TiW |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|W-TiW Deposition (Sputter 4)}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!MnS |
|||
! bgcolor="#d0e7ff" align="center" | TiO<sub>2</sub> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E2}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | {{Rl|Sputtering Recipes|TiO2 deposition (Sputter 2)}} |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|Sputter 4 (AJA ATC 2200-V)}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering_Recipes#TiO2_deposition_.28IBD.29|R]] |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | {{rl|Atomic Layer Deposition Recipes|TiO2 deposition (ALD)}} |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Mo |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| <br> |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| <br> |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| <br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| [[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| [[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" | |
|||
| <br> |
|||
| bgcolor="#eeffff" | |
|||
| <br> |
|||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
| bgcolor="#eeffff" |<br> |
||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
!Na |
|||
! bgcolor="#d0e7ff" align="center" | W |
|||
| |
|||
| bgcolor="#eeffff" | {{Al/E1}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | [[Sputtering Recipes|A]] |
|||
| |
|||
| bgcolor="#eeffff" | {{rl|Sputtering Recipes|W deposition (Sputter 4)}} |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!NaCl |
|||
! bgcolor="#d0e7ff" align="center" | Zn |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| [[Thermal Evaporation Recipes|A]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Nb |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | {{rl|Atomic Layer Deposition Recipes|ZnO deposition (ALD)}} |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
!NbO5 |
|||
! bgcolor="#d0e7ff" align="center" | Zr |
|||
| |
|||
| {{Al/E1}} |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| {{Al/E4}} |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| [[Sputtering Recipes|A]] |
|||
| |
|||
| [[Sputtering Recipes|A]] |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| |
|||
| <br> |
|||
| <br> |
|||
| <br> |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" | |
! bgcolor="#d0e7ff" align="center" |Nd |
||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
| |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
|<br> |
|||
| bgcolor="#eeffff" | <br> |
|||
| bgcolor="#eeffff" | {{rl|Atomic Layer Deposition Recipes|ZrO2 deposition (ALD)}} |
|||
| bgcolor="#eeffff" | <br> |
|||
|- |
|- |
||
! |
! bgcolor="#d0e7ff" align="center" |Ni |
||
| |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
|||
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]] |
|||
| |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
||
| |
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ni|R6]] |
||
| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |<br> |
|||
| width="65" bgcolor="#daf1ff" | [[Sputtering Recipes#Sputter_2_.28SFI_Endeavor.29|Sputter 2<br>(SFI Endeavor)]] |
|||
| bgcolor="#eeffff" |R1 |
|||
| width="65" bgcolor="#daf1ff" | [[Sputtering Recipes#Sputter_3_.28ATC_2000-F.29|Sputter 3<br>(ATC 2000-F)]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| width="65" bgcolor="#daf1ff" | [[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(ATC 2200-V)]] |
|||
| |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
|||
| width="55" bgcolor="#daf1ff" | [[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| width="45" bgcolor="#daf1ff" | [[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| width="65" bgcolor="#daf1ff" | [[Thermal Evaporation Recipes#Thermal_Evap_2_.28Solder.29|Thermal Evap 2 (Solder)]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| width="65" bgcolor="#daf1ff" | [[PECVD Recipes#PECVD_1_.28PlasmaTherm_790.29|PECVD 1<br>(PlasmaTherm 790)]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| width="65" bgcolor="#daf1ff" | [[PECVD Recipes#PECVD_2_.28Advanced_Vacuum.29|PECVD 2<br>(Advanced Vacuum)]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| width="65" bgcolor="#daf1ff" | [[PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29|Unaxis VLR ICP-PECVD]] |
|||
|- |
|||
| width="65" bgcolor="#daf1ff" | [[Atomic_Layer_Deposition_Recipes|Atomic Layer Deposition (Oxford FlexAl)]] |
|||
! bgcolor="#d0e7ff" align="center" |NiCr |
|||
| width="65" bgcolor="#daf1ff" | [[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]] |
|||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| |
|||
| |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |NiFe |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
|- |
|||
!Pb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!PbS |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Pd |
|||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|<br> |
|||
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Pt |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bcolor="EEFFFF" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Ru |
|||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|<br> |
|||
|<br> |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|<br> |
|||
|[[Sputtering Recipes#Ru Deposition .28Sputter 4.29|R3]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
|||
|<br> |
|||
|- |
|||
!Sb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!Se |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Si |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |R1 |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R3] |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |SiN |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Sputtering Recipes|R3]] |
|||
|[[Sputtering Recipes|R1]] |
|||
|<br> |
|||
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]] |
|||
|<br> |
|||
|<br> |
|||
|[[PECVD Recipes#SiN deposition .28PECVD .231.29|R6]] |
|||
|[[PECVD Recipes#SiN deposition .28PECVD .232.29|R6]] |
|||
|[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]] |
|||
|<br> |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |SiN - Low Stress |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[PECVD Recipes#Low Stress Si3N4 .28PECVD.231.29|R4]] |
|||
|[[PECVD Recipes#Low-Stress SiN deposition .28PECVD .232.29|R6]] |
|||
|[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]] |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R6]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R6]] |
|||
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]] |
|||
| bgcolor="#eeffff" |[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]] |
|||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
!SiO<sub>x</sub> |
|||
| |
|||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!SiO |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |SiO<sub>x</sub>N<sub>y</sub> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R3]] |
|||
|<br> |
|||
|<br> |
|||
|[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R4]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Sn |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |SrF<sub>2</sub> |
|||
|<br> |
|||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Ta |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |R1 |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
|||
|<br> |
|||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]] |
|||
|<br> |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]] |
|||
|<br> |
|||
| |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Ti |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ti|R6]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |R1 |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |TiN |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29 R3] |
|||
|<br> |
|||
|R1 |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |TiW |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
!TiO |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |V |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Sputtering Recipes|R1]] |
|||
|[[Sputtering Recipes|R1]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
| |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |W |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
!WC |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Zn |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |ZnO |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
!ZnS |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |Zr |
|||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|<br> |
|||
|<br> |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|[[Sputtering Recipes|R1]] |
|||
|[[Sputtering Recipes|R1]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
|||
| bgcolor="#eeffff" |<br> |
|||
|- |
|||
! width="20" bgcolor="#d0e7ff" align="center" |'''Material''' |
|||
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]] |
|||
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]] |
|||
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_3_.28Temescal.29|E-Beam 3 (Temescal)]] |
|||
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_4_.28CHA.29|E-Beam 4 (CHA)]] |
|||
| width="65" bgcolor="#daf1ff" |[[Sputtering Recipes#Sputter_3_.28ATC_2000-F.29|Sputter 3<br>(ATC 2000-F)]] |
|||
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(ATC 2200-V)]] |
|||
| width="65" bgcolor="#daf1ff" |[[Sputtering Recipes|Sputter 5 (ATC 2200-V)]] |
|||
| width="55" bgcolor="#daf1ff" |[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]] |
|||
| width="45" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]] |
|||
| width="65" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_2_.28Solder.29|Thermal Evap 2 (Solder)]] |
|||
| width="65" bgcolor="#daf1ff" |[[PECVD Recipes#PECVD_1_.28PlasmaTherm_790.29|PECVD 1<br>(PlasmaTherm 790)]] |
|||
| width="65" bgcolor="#daf1ff" |[[PECVD Recipes#PECVD_2_.28Advanced_Vacuum.29|PECVD 2<br>(Advanced Vacuum)]] |
|||
| width="65" bgcolor="#daf1ff" |[[PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29|Unaxis VLR ICP-PECVD]] |
|||
| width="65" bgcolor="#daf1ff" |[[Atomic_Layer_Deposition_Recipes|Atomic Layer Deposition (Oxford FlexAl)]] |
|||
| width="65" bgcolor="#daf1ff" |[[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]] |
|||
|} |
|} |
||
===Process Ranking Table=== |
|||
Processes in the table above are ranked by their "''Process Maturity Level''" as follows: |
|||
{| class="wikitable" |
|||
|'''Process Level''' |
|||
| colspan="11" |'''Description of Process Level Ranking''' |
|||
|- |
|||
|A |
|||
| colspan="11" |Process '''A'''llowed and materials available but never done |
|||
|- |
|||
|R1 |
|||
| colspan="11" |Process has been ran at least once |
|||
|- |
|||
|R2 |
|||
| colspan="11" |Process has been ran and/or procedure is documented or/and data available |
|||
|- |
|||
|R3 |
|||
| colspan="11" |Process has been ran, procedure is documented, and data is available |
|||
|- |
|||
|R4 |
|||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''or''' lookahead/in-Situ control available |
|||
|- |
|||
|R5 |
|||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' lookahead/in-Situ control available |
|||
|- |
|||
|R6 |
|||
| colspan="11" |Process has a documented procedure, regular ( ≥4x per year) data, and control charts/limits available |
|||
|} |
|||
[[Category:Processing]] |
[[Category:Processing]] |
||
Revision as of 17:55, 5 March 2025
Process Control Data
See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.
Deposition Tools/Materials Table
The Key/Legend for this table's R1...R6 values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
| Process Level | Description of Process Level Ranking | ||||||||||
| A | Process Allowed and materials available but never done | ||||||||||
| R1 | Process has been ran at least once | ||||||||||
| R2 | Process has been ran and/or procedure is documented or/and data available | ||||||||||
| R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
| R4 | Process has a documented procedure with regular (≥4x per year) data or lookahead/in-Situ control available | ||||||||||
| R5 | Process has a documented procedure with regular (≥4x per year) data and lookahead/in-Situ control available | ||||||||||
| R6 | Process has a documented procedure, regular ( ≥4x per year) data, and control charts/limits available | ||||||||||