Dry Etching Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(lkink change)
(updated FL-ICP Si + SIO2 link cuz changed header title)
 
(85 intermediate revisions by 7 users not shown)
Line 1: Line 1:
===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>===
{{Recipe Table Explanation}}
<small>''See above [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used dry etches''</small>

===Dry Etching Tools/Materials Table===
''The Key/Legend for this table's <code>A...R6</code> values is at the [[Dry Etching Recipes#Process Ranking Table|bottom of the page]].''
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
|-
! colspan="15" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
| bgcolor="#eaecf0" |<!-- INTENTIONALLY LEFT BLANK -->
! colspan="18" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
! colspan="2" |'''[[RIE Etching Recipes|RIE Etching]]'''
|- bgcolor="#d0e7ff"
|<!-- INTENTIONALLY LEFT BLANK -->
! colspan="4" width="300" height="35" align="center" bgcolor="#d0e7ff" |'''[[RIE Etching Recipes|RIE Etching]]'''
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="5" align="center" bgcolor="#d0e7ff" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="4" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="3" align="center" bgcolor="#d0e7ff" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
|- bgcolor="#d0e7ff"
|-
! width="65" align="center" bgcolor="#d0e7ff" |'''Material'''
! bgcolor="#d0e7ff" align="center" |'''Material'''
| width="65" bgcolor="#daf1ff" |[[RIE 1 (Custom)|RIE 1<br>(Retired)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| width="100" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| width="100" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E646V)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| width="100" bgcolor="#daf1ff" |[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#PlasmaTherm.2FSLR_Fluorine_Etcher SLR Fluorine ICP (PlasmaTherm)]
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic 1)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic 2)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
| width="85" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| width="95" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]]
| width="95" bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean (YES EcoClean)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Ag
! bgcolor="#d0e7ff" align="center" |Ag
|
|
|
|
Line 43: Line 44:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Al
|
|
|[[RIE Etching Recipes|R2]]
|
|
|
|
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)|R1}}
|[[ICP Etching Recipes#Al Etch .28Panasonic 2.29|R2]]
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Al
|
|
|
|
|
|
|[[RIE Etching Recipes|A]]
|
|
|
|
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 2)}}
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Au
|
|
|
|
Line 65: Line 70:
|
|
|
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Au
|
|
|
|
Line 74: Line 76:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Cr
|
|
|[[RIE Etching Recipes|R2]]
|
|
|
|
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}}
|R1
|
|
|
|
Line 84: Line 92:
|
|
|
|
|R1
|[https://www.nanotech.ucsb.edu/wiki/index.php/Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29 A]
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Cr
! bgcolor="#d0e7ff" align="center" |Cu
|
|
|
|
|
|
|A
|
|
|
|
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}}
|A
|
|
|
|
Line 103: Line 108:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ge
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Cu
|
|
|
|
|
|
|A
|R1
|
|
|
|
Line 114: Line 122:
|
|
|
|
|[[Other Dry Etching Recipes|R2]]
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Mo
|
|
|
|
Line 123: Line 135:
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |Ge
|
|
|
|
Line 130: Line 140:
|
|
|
|
|R1
|-
!Nb
|
|
|
|
|
|
|
|
|A
|R1
|
|
|
|
|
|
|
|
|
|A
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Mo
|
|
|
|
|
|
|
|
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ni
|
|
|
|
Line 161: Line 172:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|-
|-
!Os
! align="center" bgcolor="#d0e7ff" |Ni
|
|
|
|
|
|
|
|
|A
|R1
|
|
|
|
Line 175: Line 189:
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Pt
|
|
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
! align="center" bgcolor="#d0e7ff" |Pt
|
|
|
|
Line 191: Line 204:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ru
|
|
|
|
|
|
|
|
|A
|[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R3]]
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
! align="center" bgcolor="#d0e7ff" |Ru
|
|
|
|
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Si
|
|
|
|
|[[ICP Etching Recipes#DSEIII .28PlasmaTherm.2FDeep Silicon Etcher.29|R6]]
|A
|{{Rl|ICP Etching Recipes|Ru (Ruthenium) Etch (Panasonic 2)}}
|[[ICP Etching Recipes#Si Etch Recipes (Fluorine ICP Etcher)|R6]]
|
|
|
|
|R1
|
|
|
|
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ta
|
|
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Si
|
|
|
|
|A
|R1
|
|
|
|
|{{rl|ICP Etching Recipes|DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)}}
|{{Rl|ICP Etching Recipes|Si Etching}}
|
|
|
|
Line 231: Line 252:
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ti
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
|
|
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}}
|
|-
|R1
! align="center" bgcolor="#d0e7ff" |Ta
|
|
|
|
Line 246: Line 268:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |W
|
|
|
|
|
|
|R2
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}}
|R1
|
|
|
|
Line 256: Line 284:
|
|
|
|
|R1
|-
|-
!TiW
! align="center" bgcolor="#d0e7ff" |Ti
|
|
|
|
|
|
|R2
|
|
|R1
|
|
|
|
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}}
|A
|
|
|
|
Line 272: Line 301:
|
|
|
|
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
|
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3</sub>
|
|
|
|
|
|
|
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|
|
|
|
|A
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]]
|
|
|
|
Line 294: Line 316:
|
|
|
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
|
|
|
|
|
|
Line 303: Line 324:
|
|
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}}
|A
|R1
|
|
|
|
Line 311: Line 332:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |AlGaAs
|
|
|[[RIE Etching Recipes|R3]]
|
|
|-
! align="center" bgcolor="#d0e7ff" |AlGaAs
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}}
|
|
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]]
|
|
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|
|
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}}
|
|
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}}
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |AlGaN
|
|
|
|
Line 332: Line 357:
|
|
|
|
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R2]]
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |AlGaN
|
|
|
|
Line 340: Line 364:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |AlN
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
Line 351: Line 377:
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |AlN
|
|
|
|
|
|
|R1
|-
!BCB
|
|
|
|
|
|
|
|
|A
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
Line 371: Line 398:
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |CdZnTe
! bgcolor="#d0e7ff" align="center" |CdZnTe
|[[RIE Etching Recipes|R3]]
|
|
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
|
|
|
|
Line 385: Line 412:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |GaAs
|
|
|[[RIE Etching Recipes|R4]]
|
|
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}}
|[[ICP Etching Recipes#GaAs Etch .28Panasonic 2.29|R6]]
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R2]]
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |GaAs
|
|
|
|
|
|
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|
|
|R1
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}}
|- bgcolor="#eeffff"
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}}
! bgcolor="#d0e7ff" align="center" |GaN
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}}
|
|
|[[RIE Etching Recipes|R4]]
|
|
|
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |GaN
|
|
|
|{{rl|RIE Etching Recipes|GaN Etching (RIE 5)}}
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
|R1
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R6]]
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
Line 424: Line 444:
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
|
! bgcolor="#d0e7ff" align="center" |GaSb
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |GaSb
|
|
|
|
|
|
|
Line 437: Line 452:
|
|
|A
|A
|R1
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
|
|R1
|
|
|
|
|
Line 446: Line 460:
|
|
|
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |HfO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub>
|
|
|
|
Line 461: Line 476:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |InGaAlAs
|[[RIE Etching Recipes|R4]]
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |InGaAlAs
|
|
|R1
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
Line 475: Line 492:
|
|
|
|
|R1
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |InGaAsP
|[[RIE Etching Recipes|R4]]
|
|
|
|
Line 481: Line 501:
|
|
|
|
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R3]]
|
|
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |InGaAsP
|
|
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |InP
|[[RIE Etching Recipes|R4]]
|
|
|
|
|
|
|
|A
|R1
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R6]]
|
|
|
|
|
|
Line 503: Line 524:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |InP
! bgcolor="#d0e7ff" align="center" |ITO
|[[RIE Etching Recipes|R4]]
|
|
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
|
|
|
|A
|A
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
Line 522: Line 540:
|
|
|
|
|R1
|-
|-
!LiNbO3
! align="center" bgcolor="#d0e7ff" |ITO
|
|
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
|
|
|
|
Line 538: Line 556:
|
|
|
|
|R1
|- bgcolor="#ffffff"
!Photoresist & Organics
|
|
|[[RIE Etching Recipes|R3]]
|
|
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]]
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R]
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]]
|
|
|R3
|- bgcolor="#eeffff"
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
!Photoresist
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
& ARC
|
|
|
|
|A
|[https://www.nanotech.ucsb.edu/wiki/index.php/RIE_Etching_Recipes#Photoresist_and_ARC R]
|
|
|R1
|-
!ARC (Anti Reflective Coating)
|
|
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_Etching R]
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_etching_2 R]
|
|
|A
|A
|
|
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]]
|
|
|
|
Line 561: Line 584:
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |SiC
|
|
|
|
Line 568: Line 589:
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |SiC
|
|
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}}
|A
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}}
|R1
|
|
|
|
Line 580: Line 603:
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |SiN
|
|
|
|R1
|- bgcolor="#ffffff"
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
! bgcolor="#d0e7ff" align="center" |SiN
|
|
|
|
|
|
|[[ICP Etching Recipes#Si3N4 Etching .28Fluorine ICP Etcher.29|R3]]
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}}
|[[ICP Etching Recipes#SiNx Etching .28Panasonic 2.29|R3]]
|
|A
|
|
|
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
|
|
|
|
Line 599: Line 620:
|
|
|
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |SiO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
|
|
|
|
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
|
|
|[[ICP Etching Recipes#SiO2 Etch Recipes (Fluorine ICP Etcher)|R6]]
|
|A
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
|[[ICP Etching Recipes#SiO2 Etching .28Panasonic 2.29|R6]]
|
|
|
|
Line 615: Line 635:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |SiOxNy
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |SiOxNy
|
|
|
|
|
|
|
|
|A
|A
|A
|R1
|
|
|
|
Line 635: Line 652:
|
|
|
|
|
|R1
|
|-
|-
!SU8
! align="center" bgcolor="#d0e7ff" |Ta<sub>2</sub>O<sub>5</sub>
|
|
|
|
|
|
|
|
|A
|
|
|
|
|
|
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A]
|
|
|
|
Line 653: Line 669:
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
|
|
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |TiN
|
|
|A
|R1
|
|
|
|
Line 666: Line 684:
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
|
! bgcolor="#d0e7ff" align="center" |TiN
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |TiO<sub>2</sub>
|
|
|
|
|
|
|
|
Line 694: Line 700:
|
|
|
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |W-TiW
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
|
|
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}}
|A
|
|
|
|
Line 713: Line 716:
|
|
|
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |ZnO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub>
|
|
|
|
Line 728: Line 732:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |ZnS
|[[RIE Etching Recipes|R3]]
|
|
|
|
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |ZnS
|
|
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|
|
|
|
Line 743: Line 748:
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |ZnSe
|[[RIE Etching Recipes|R2]]
|
|
|
|
Line 751: Line 760:
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |ZnSe
|
|
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub>
|
|
|
|
Line 770: Line 779:
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |ZrO<sub>2</sub>
|
|
|
|R1
|- bgcolor="#eeffff"
|
! bgcolor="#d0e7ff" align="center" |'''Material'''
|
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
|
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
|
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
|
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
|
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
|
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]]
|
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
|
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
|
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
|
|
|
|
|
|-
! align="center" bgcolor="#d0e7ff" |'''Material'''
| bgcolor="#daf1ff" |[[RIE 1 (Custom)|RIE 1<br>(Retired)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|SLR Fluorine ICP (PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic E626I)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic E640)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| bgcolor="#daf1ff" |[[Plasma Clean (YES EcoClean)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]]
|}
|}


==='''Process Ranking Table'''===
Processes in the table above are ranked by their "''Process Maturity Level''" as follows:
{| class="wikitable"
!Process Level
! colspan="11" |Description of Process Level Ranking
|-
|A
| colspan="11" |Process '''A'''llowed and materials available but never done
|-
|R1
| colspan="11" |Process has been run at least once
|-
|R2
| colspan="11" |Process has been run and/or procedure is documented or/and data available
|-
|R3
| colspan="11" |Process has been run, procedure is documented, and data is available
|-
|R4
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''or''' lookahead/in-situ control available
|-
|R5
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' lookahead/in-situ control available
|-
|R6
| colspan="11" |Process has a documented procedure, regular ( ≥4x per year) data, and control charts & limits available
|}
[[Category:Processing]]
[[Category:Processing]]

Latest revision as of 18:55, 9 March 2025

Process Control Data

See above linked page for process control data (dep rate/stress etc. over time), for a selection of often-used dry etches

Dry Etching Tools/Materials Table

The Key/Legend for this table's A...R6 values is at the bottom of the page.

Dry Etching Recipes
RIE Etching ICP Etching Oxygen Plasma Systems Other Dry Etchers
Material RIE 2
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E646V)
ICP Etch 2
(Panasonic E626I)
Oxford ICP (PlasmaPro 100) Ashers
(Technics PEII)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)
Ag R1
Al R2 R1 R2 R1
Au R4
Cr R2 R1 R1 R1
Cu R1
Ge A R1 R2 R1
Mo R1
Nb A R1
Ni R4
Os A R1
Pt R4
Ru A R3 R1
Si R6 R6 R1 R4 R1
Ta A R1 R1
Ti R1 R1 R1
W R2 R1 R1 R1
TiW R2 R1
Al2O3 A R3 R1
Al2O3 (Sapphire) R1 R1 R1
AlGaAs R3 R1 R3 R1
AlGaN R2 R1
AlN R1
BCB A
CdZnTe R3 R1
GaAs R4 R1 R6 R2 R1
GaN R4 R1 R1 R6 R1
GaSb A R1 R1 R1
HfO2 R1
InGaAlAs R4 R1 R1
InGaAsP R4 R3 R1
InP R4 A R1 R6 R4
ITO R4 R1
LiNbO3 R1
Photoresist & Organics R3 R3 R R3 R3 R3 R3 R1
ARC (Anti Reflective Coating) R3
SiC R1 R1 R1
SiN R3 R1 R3 R3 R1
SiO2 R6 R1 R6 R4 R1
SiOxNy A R1 R1
SU8 A
Ta2O5 A R1 R1
TiN R1
TiO2 R1
ZnO2 R1
ZnS R3 R1
ZnSe R2 R1
ZrO2 R1
Material RIE 2
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
Oxford ICP (PlasmaPro 100) Ashers
(Technics PEII)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)

Process Ranking Table

Processes in the table above are ranked by their "Process Maturity Level" as follows:

Process Level Description of Process Level Ranking
A Process Allowed and materials available but never done
R1 Process has been run at least once
R2 Process has been run and/or procedure is documented or/and data available
R3 Process has been run, procedure is documented, and data is available
R4 Process has a documented procedure with regular (≥4x per year) data or lookahead/in-situ control available
R5 Process has a documented procedure with regular (≥4x per year) data and lookahead/in-situ control available
R6 Process has a documented procedure, regular ( ≥4x per year) data, and control charts & limits available