Vacuum Deposition Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
m add Sputter5 ITO and Ni currently on system |
→Process Ranking Table: adding to R4 definition |
||
| (26 intermediate revisions by 3 users not shown) | |||
| Line 3: | Line 3: | ||
===Deposition Tools/Materials Table=== |
===Deposition Tools/Materials Table=== |
||
''The Key/Legend for this table's <code>A...R6</code> values is at the [[Vacuum Deposition Recipes#Process Ranking Table|<u>bottom of the page</u>]].'' |
|||
==== Process Maturity Ranking ==== |
|||
* <code>'''R6'''</code> - most mature process with regular calibrations recorded on SPC charts. |
|||
* … |
|||
* <code>'''R1'''</code> - least mature - "possible" but you'll have to figure it out. |
|||
''The Key/Legend for this table's <code>R1...R6</code> values is at the [[Vacuum Deposition Recipes#Process Ranking Table|<u>bottom of the page</u>]].'' |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
| Line 41: | Line 48: | ||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
||
| Line 91: | Line 98: | ||
|[[Sputtering Recipes|R1]] |
|[[Sputtering Recipes|R1]] |
||
|[[Sputtering Recipes|R3]] |
|[[Sputtering Recipes|R3]] |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R6]] |
||
|R1 |
|R1 |
||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
| Line 109: | Line 116: | ||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29| |
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| Line 115: | Line 122: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29| |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!As |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
!AuPd |
!AuPd |
||
| Line 217: | Line 207: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29| |
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R3]] |
||
|<br> |
|<br> |
||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Au |
! bgcolor="#d0e7ff" align="center" |Au |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29| |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R6]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
||
| bgcolor="#eeffff" |[[ |
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Au|R6]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" |R2 |
|||
| bgcolor="#eeffff" |R3 |
| bgcolor="#eeffff" |R3 |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
| Line 253: | Line 243: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|- |
|||
!Be |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |C |
! bgcolor="#d0e7ff" align="center" |C |
||
| Line 287: | Line 260: | ||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
|- |
|||
!Cd |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!CdS |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!CdTe |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
!CaF2 |
!CaF2 |
||
| Line 391: | Line 313: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Cr |
! bgcolor="#d0e7ff" align="center" |Cr |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29| |
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R6]] |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[ |
|[[Process Group - Process Control Data#E-Beam 4: Cr|R6]] |
||
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R3] |
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R3] |
||
|<br> |
|<br> |
||
|{{Rl|Sputtering_Recipes|Sputter_5_.28AJA_ATC_2200-V.29| |
|{{Rl|Sputtering_Recipes|Sputter_5_.28AJA_ATC_2200-V.29|R6}} |
||
|<br> |
|<br> |
||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
| Line 440: | Line 362: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|- |
|||
!Ga |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!GaAs |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ge |
! bgcolor="#d0e7ff" align="center" |Ge |
||
| Line 494: | Line 382: | ||
! bgcolor="#d0e7ff" align="center" |GeO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |GeO<sub>2</sub> |
||
| |
| |
||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29| |
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]] |
||
| |
| |
||
| |
| |
||
| Line 548: | Line 436: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
|[[Sputtering Recipes|R1]] |
|||
| |
|||
|[[Sputtering Recipes|R1]] |
|||
|R1 |
|||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| Line 557: | Line 445: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29| |
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R3]] |
||
|<br> |
|<br> |
||
|- |
|- |
||
| Line 593: | Line 481: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!InSb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ir |
! bgcolor="#d0e7ff" align="center" |Ir |
||
| Line 630: | Line 501: | ||
! bgcolor="#d0e7ff" align="center" |ITO |
! bgcolor="#d0e7ff" align="center" |ITO |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29| |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R4]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| Line 867: | Line 738: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ni |
! bgcolor="#d0e7ff" align="center" |Ni |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29| |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R6]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
||
| bgcolor="#eeffff" |[[ |
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ni|R6]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| Line 916: | Line 787: | ||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
|- |
|||
!Pb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!PbS |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Pd |
! bgcolor="#d0e7ff" align="center" |Pd |
||
| Line 956: | Line 793: | ||
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
||
|[[Sputtering Recipes|R1]] |
|||
|<br> |
|||
|[[Sputtering Recipes|R1]] |
|||
|<br> |
|||
|R1 |
|||
|<br> |
|||
|<br> |
|<br> |
||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
| Line 982: | Line 819: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29| |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|- |
||
| Line 999: | Line 836: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29| |
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
||
|<br> |
|<br> |
||
|- |
|||
!Sb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!Se |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Si |
! bgcolor="#d0e7ff" align="center" |Si |
||
| Line 1,081: | Line 884: | ||
| |
| |
||
| |
| |
||
|[[PECVD Recipes#Low Stress Si3N4 .28PECVD.231.29| |
|[[PECVD Recipes#Low Stress Si3N4 .28PECVD.231.29|R3]] |
||
|[[PECVD Recipes#Low-Stress SiN deposition .28PECVD .232.29|R6]] |
|[[PECVD Recipes#Low-Stress SiN deposition .28PECVD .232.29|R6]] |
||
|[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]] |
|[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]] |
||
| |
|||
| |
|||
|- |
|||
!SiN - Low Stress 3xTime |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[PECVD Recipes#Low-Stress SiN 3xTime (PECVD #2)|R6]] |
|||
| |
|||
| |
| |
||
| |
| |
||
| Line 1,101: | Line 921: | ||
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]] |
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]] |
||
| bgcolor="#eeffff" |[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]] |
| bgcolor="#eeffff" |[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]] |
||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29| |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!SiO<sub>x</sub> |
|||
| |
|||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
!SiO |
!SiO |
||
| Line 1,149: | Line 952: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[PECVD Recipes#SiO2 deposition .28PECVD .231.29| |
|[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R3]] |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| Line 1,210: | Line 1,013: | ||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]] |
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]] |
||
|<br> |
|<br> |
||
| |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| Line 1,224: | Line 1,027: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ti |
! bgcolor="#d0e7ff" align="center" |Ti |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29| |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R6]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
||
| bgcolor="#eeffff" |[[ |
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ti|R6]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R6]] |
|||
| bgcolor="#eeffff" |R1 |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| Line 1,246: | Line 1,049: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Sputtering Recipes#Sputter 4 (AJA ATC 2200-V)|R3]] |
|||
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29 R3] |
|||
|<br> |
|<br> |
||
|R1 |
|R1 |
||
| Line 1,254: | Line 1,057: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29| |
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
||
|<br> |
|<br> |
||
|- |
|- |
||
| Line 1,262: | Line 1,065: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes#TiW Co-Sputter Deposition (Sputter 3)|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| Line 1,273: | Line 1,076: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!TiO |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
||
| Line 1,299: | Line 1,085: | ||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29| |
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| Line 1,305: | Line 1,091: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29| |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|- |
||
| Line 1,330: | Line 1,116: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes#TiW Co-Sputter Deposition (Sputter 3)|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| Line 1,392: | Line 1,178: | ||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!ZnS |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Zr |
! bgcolor="#d0e7ff" align="center" |Zr |
||
| Line 1,441: | Line 1,210: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29| |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|- |
||
| Line 1,465: | Line 1,234: | ||
Processes in the table above are ranked by their "''Process Maturity Level''" as follows: |
Processes in the table above are ranked by their "''Process Maturity Level''" as follows: |
||
{| class="wikitable" |
{| class="wikitable" |
||
!Process Level |
|||
! colspan="11" |Description of Process Level Ranking |
|||
|- |
|- |
||
|A |
|A |
||
| colspan="11" |Process '''A'''llowed and materials available but never |
| colspan="11" |Process '''A'''llowed and materials available but never done |
||
|- |
|- |
||
|R1 |
|R1 |
||
| Line 1,475: | Line 1,244: | ||
|- |
|- |
||
|R2 |
|R2 |
||
| colspan="11" |Process has been ran and |
| colspan="11" |Process has been ran and procedure is documented |
||
|- |
|- |
||
|R3 |
|R3 |
||
| Line 1,481: | Line 1,250: | ||
|- |
|- |
||
|R4 |
|R4 |
||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data ''' |
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''no''' in-Situ control available |
||
|- |
|- |
||
|R5 |
|R5 |
||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' |
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' in-Situ control available |
||
|- |
|- |
||
|R6 |
|R6 |
||
| colspan="11" |Process has a documented procedure |
| colspan="11" |Process has a documented procedure and control charts/limits available. Controlled process. |
||
|} |
|} |
||
[[Category:Processing]] |
[[Category:Processing]] |
||
Revision as of 19:59, 22 August 2025
Process Control Data
See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.
Deposition Tools/Materials Table
Process Maturity Ranking
R6- most mature process with regular calibrations recorded on SPC charts.- …
R1- least mature - "possible" but you'll have to figure it out.
The Key/Legend for this table's R1...R6 values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
| Process Level | Description of Process Level Ranking | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| A | Process Allowed and materials available but never done | ||||||||||
| R1 | Process has been ran at least once | ||||||||||
| R2 | Process has been ran and procedure is documented | ||||||||||
| R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
| R4 | Process has a documented procedure with regular (≥4x per year) data no in-Situ control available | ||||||||||
| R5 | Process has a documented procedure with regular (≥4x per year) data and in-Situ control available | ||||||||||
| R6 | Process has a documented procedure and control charts/limits available. Controlled process. | ||||||||||