Vacuum Deposition Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
No edit summary |
→Process Ranking Table: adding to R4 definition |
||
| Line 1,250: | Line 1,250: | ||
|- |
|- |
||
|R4 |
|R4 |
||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data |
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''no''' in-Situ control available |
||
|- |
|- |
||
|R5 |
|R5 |
||
Latest revision as of 19:59, 22 August 2025
Process Control Data
See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.
Deposition Tools/Materials Table
Process Maturity Ranking
R6- most mature process with regular calibrations recorded on SPC charts.- …
R1- least mature - "possible" but you'll have to figure it out.
The Key/Legend for this table's R1...R6 values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
| Process Level | Description of Process Level Ranking | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| A | Process Allowed and materials available but never done | ||||||||||
| R1 | Process has been ran at least once | ||||||||||
| R2 | Process has been ran and procedure is documented | ||||||||||
| R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
| R4 | Process has a documented procedure with regular (≥4x per year) data no in-Situ control available | ||||||||||
| R5 | Process has a documented procedure with regular (≥4x per year) data and in-Situ control available | ||||||||||
| R6 | Process has a documented procedure and control charts/limits available. Controlled process. | ||||||||||