{{recipes|Vacuum Deposition}} |
{{recipes|Vacuum Deposition}} |
||
=[[PECVD 1 (PlasmaTherm 790)]]= |
=[[PECVD 1 (PlasmaTherm 790)]]= |
||
*[https://docs.google.com/spreadsheets/d/1a0XrY6HuJ6L9niThZYI-u4XH69Hnbe3jkm1qKmrR8Rg/edit#gid=sharing Particulates in PECVD 1] |
|||
== SiN deposition (PECVD #1) == |
|||
*[[media:New PECVD1-SiO2-standard recipe 2014 SiO2 standard recipe.pdf|SiN Standard Recipe]] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN Data 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1phx1WficlUEg0xSahaAq4zrRk6m9Eb0ausO8wcAmXqs/edit#gid=sharing SiN Data 2015] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 1000A Thickness uniformity 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1-pET1Eojooso5UHk90W-5uYByDDdrCyRnggqewxTmVg/edit#gid=sharing SiN 1000A Thickness uniformity 2015] |
|||
<!-- Placeholders - Not uploaded yet--> |
|||
===[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1270764394 PECVD 1 Process Control Plots] - Plots of all process control data=== |
|||
*[[media:New PECVD1-LS SIN-Turner05recipe 2014 LS SIN recipe.pdf|LS SiN Standard Recipe]] |
|||
*[https://docs.google.com/spreadsheets/d/1Joz0az9TGZWQc4CiMQJZzLBbNFbx_hH2Oc0B4NNJmYk/edit#gid=sharing LS SiN Data 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1xIzc2CufRYNSfAtsOXpw3IzHreeu42BWrLBV0kzP6kA/edit#gid=sharing LS SiN 1000A Thickness uniformity 2014] |
|||
<!-- Placeholders - Not uploaded yet--> |
|||
== |
==SiO<sub>2</sub> deposition (PECVD #1)== |
||
*[[media:New PECVD1-SiN-standard recipe 2014 SiN standard recipe.pdf|SiO<sub>2</sub> Standard Recipe]] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEw0bjFEdTF2SUhRa25Ca0d0SzBha3c&usp=drive_web#gid=sharing SiO<sub>2</sub> Data 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1JWNUcH8l90xif-0BhYKJee9nXxE4hnvvp6N2NtZLYXY/edit#gid=sharing SiO<sub>2</sub> Data 2015] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDQ3VEtZQVRpdVdlbGtIZHpTNmFzNmc&usp=drive_web#gid=sharing SiO<sub>2</sub> 1000A Thickness uniformity 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1NQy-ADou6f2NBU-9jZG8KME1lOz0X5mh6HZV9_jPGes/edit#gid=sharing SiO<sub>2</sub> 1000A Thickness uniformity 2015] |
|||
*[https://docs.google.com/spreadsheets/d/1wloq6HJw5RQIvmeKcBn3xvE_917R6jF_K-btCHjsiIM/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
|||
== SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1) == |
|||
<!-- Placeholders - Not uploaded yet--> |
|||
*[[media:New PECVD1-LS SION-recipe 2014 LS SION recipe.pdf|SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]] |
|||
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
|||
=[[PECVD 2 (Advanced Vacuum)]]= |
|||
**Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
*[https://docs.google.com/spreadsheets/d/1kj0SWxRpnPRoGld8k3sW-3yK1iPm3buTkvlJSN5YPV4/edit#gid=sharing Particulates in Advanced PECVD ] |
|||
== SiO<sub>2</sub> deposition (PECVD #2) == |
|||
*[[media:New Adv PECVD OXIDE 300C standard recipe OXIDE Standard Recipe.pdf|Oxide Standard Recipe]] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1d5boeJRWWgMqvQe6nVM7m8s3KAcS4Yp2L5CEU9svkX4/edit#gid=sharing Oxide Data 2015] |
|||
*[https://docs.google.com/spreadsheets/d/1XQRcTJdw9AIMPAUsH0n9Ic9Fe1_xGDSvAxD4gVc9FBw/edit#gid=sharing Oxide data 2016] |
|||
=== Old Data === |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness Uniformity 2014] |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.231.29 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier |
|||
*[https://docs.google.com/spreadsheets/d/16pZHcGwesXB1mMPwntOudBIlPvRh6A6DI37DEwyYfPw/edit#gid=sharing Oxide Thickness Uniformity 2015] |
|||
== |
==SiN deposition (PECVD #1)== |
||
*[[media:New Adv PECVD-Nitride2 300C standard recipe Nitride2 Standard Recipe.pdf|Nitride2 Standard Recipe]] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1SkYqOwgjUyMaFBPhuTjMvBTXu0KdQFNmITryF_OVi8o/edit#gid=sharing Nitride2 Data 2015] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness Uniformity 2014] |
|||
*[https://docs.google.com/spreadsheets/d/14_dYQu3z31fF_oxsUUX8BmDucgv6B07xB3_zqP0HmvM/edit#gid=sharing Nitride2 Thickness Uniformity 2015] |
|||
*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
|||
==LS SiN deposition (PECVD #2) == |
|||
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=98787450 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
|||
**Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
=== Old Data === |
|||
*[[media:New Adv PECVD-LS Nitride2 300C standard recipe LS Nitride2 standard recipe.pdf|LS Nitride2 Standard Recipe]] |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.231.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014] |
|||
*[https://docs.google.com/spreadsheets/d/16Q6BrPoNiFP0elVoSGwXRfQdHXzAXOgiyqKmEw-4kII/edit#gid=sharing LS Nitride2 data 2015] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness Uniformity 2014] |
|||
*[https://docs.google.com/spreadsheets/d/1LpkaOpr7oNoyvxFkineD7i9FspO6LweJMulvZHJM5Zc/edit#gid=sharing LS Nitride2 Thickness Uniformity 2015] |
|||
== |
==Low Stress Si<sub>3</sub>N<sub>4</sub> (PECVD#1)== |
||
*[[media:03-Amorphous-Si-PECVD-2.pdf|Amorphous Si Deposition Recipe]] |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
|||
= [[ICP-PECVD (Unaxis VLR)]] = |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#Low-Stress_SiN_-_LS-SiN_.28PECVD.231.29 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - 2021-10 and earlier |
|||
==SiN deposition (Unaxis VLR) == |
|||
=== SiN (2% SiH<sub>4</sub>) === |
|||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
|- bgcolor="#D0E7FF" |
|||
!width=350 align=center|50° (pinholes) |
|||
!width=350 align=center|100° (pinholes) |
|||
!width=350 align=center|250° |
|||
|-align=left |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-5W-50C-High-Stress.pdf|SiN Deposition Recipe (5W 50° High Stress)]] |
|||
*[[Media:PECVD2-SiN-Recipe-50W-50C-Medium-Stress.pdf|SiN Deposition Recipe (50W 50° Medium Stress)]] |
|||
*[[Media:PECVD2-SiN-Recipe-120W-50C-Low-Stress.pdf|SiN Deposition Recipe (120W 50° Low Stress)]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-5W-100C-High-Stress.pdf|SiN Deposition Recipe (5W 100° High Stress)]] |
|||
*[[Media:PECVD2-SiN-Recipe-50W-100C-Medium-Stress.pdf|SiN Deposition Recipe (50W 100° Medium Stress)]] |
|||
*[[Media:PECVD2-SiN-Recipe-120W-100C-Low-Stress.pdf|SiN Deposition Recipe (120W 100° Low Stress)]] |
|||
*[[Media:PECVD2-SiNx-l.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (120W 100° Low Stress)]] |
|||
*[[Media:PECVD2-SiNx-medium-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (50W 100° Medium Stress)]] |
|||
*[[Media:PECVD2-SiNx -h.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (5W 100° High Stress)]] |
|||
*[[Media:PECVD2-SiNx-medium stress-SEM-2% SiH4-100C-50W.pdf|SiNx SEM images (50W 100° Medium Stress)]] |
|||
*[[Media:PECVD2-SiNx-high stress-SEM-2% SiH4-100C-5W.pdf|SiNx SEM images (5W 100° High Stress)]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-5W-250C-High-Stress.pdf|SiN Deposition Recipe (5W 250° High Stress)]] |
|||
*[[Media:PECVD2-SiN-Recipe-50W-250C-Medium-Stress.pdf|SiN Deposition Recipe (50W 250° Medium Stress)]] |
|||
*[[Media:PECVD2-SiN-Recipe-120W-250C-Low-Stress.pdf|SiN Deposition Recipe (120W 250° Low Stress)]] |
|||
*[[Media:PECVD2-SiNx-l.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (120W 250° Low Stress)]] |
|||
*[[Media:PECVD2-SiNx-medium-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (50W 250° Medium Stress)]] |
|||
*[[Media:PECVD2-SiNx -h.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (5W 250° High Stress)]] |
|||
*[[Media:28-Very-low-pin-hole-density_SiNx_film_at_300_C.pdf|Very-Low-Pin-Hole-Density SiNx Recipe(25W 300°)]] |
|||
|- |
|||
|} |
|||
:[[File:PECVD1 SiN Stress vs. N2 plot.jpg|alt=plot of SiN stress and Refractive Index vs. N2 flow. |none|thumb|414x414px|Example of Si<sub>3</sub>N<sub>4</sub> modified stress via. varying N<sub>2</sub> flow. Refractive index is relatively constant (one outlier), and stress varies continuously from tensile to compressive. ([[Demis D. John]] 2011, [https://engineering.ucsb.edu/people/daniel-blumenthal Blumenthal Group])]] |
|||
=== SiN (2% SiH<sub>4</sub> - No-Ar) === |
|||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
|- bgcolor="#D0E7FF" |
|||
!width=350 align=center|50° (pinholes) |
|||
!width=350 align=center|100° (pinholes) |
|||
!width=350 align=center|250° |
|||
|-align=left |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-5W-50C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 50° High Stress)]] |
|||
*[[Media:41-High-stress_SiNx_at_50_C_using_Unaxis_ICP_deposition_tool.pdf|Film Properties of High-stress SiN<sub>x</sub> (No Ar, 5W, 50°)]] |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-50W-50C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 50° Medium Stress)]] |
|||
*[[Media:36-Medium-stress_SiNx_using_Unaxis_ICP_deposition_tool-a.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 50°)]] |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-120W-50C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 50° Low Stress)]] |
|||
*[[Media:40-Low-stress_SiNx_at_50_C_using_Unaxis_ICP_deposition_tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 50°)]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-5W-100C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 100° High Stress)]] |
|||
*[[Media:38-High-stress_SiNx_at_100_C_using_Unaxis_ICP_deposition_tool.pdf|Film Properties of high-stress SiN<sub>x</sub> (No Ar, 5W, 100°)]] |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-50W-100C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 100° Medium Stress)]] |
|||
*[[Media:39-Medium-stress_SiNx_at_100C_using_Unaxis_ICP_deposition_tool.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 100°)]] |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-120W-100C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 100° Low Stress)]] |
|||
*[[Media:37-Low-stress_SiNx_at_100_C_using_Unaxis_ICP_deposition_tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 100°)]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-5W-250C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 250° High Stress)]] |
|||
*[[Media:34-High-stress_SiNx_at_250_C_using_Unaxis_ICP_deposition_tool.pdf|Film Properties of High-stress SiN<sub>x</sub> (No Ar, 5W, 250°)]] |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-50W-250C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 250° Medium Stress)]] |
|||
*[[Media:36-Medium-stress_SiNx_using_Unaxis_ICP_deposition_tool-a.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 250°)]] |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-120W-250C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 250° Low Stress)]] |
|||
*[[Media:35-Low-stress_SiNx_at_250_C_using_Unaxis_ICP_deposition_tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 250°)]] |
|||
|- |
|||
|} |
|||
== |
==SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1)== |
||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
|- bgcolor="#D0E7FF" |
|||
!width=350 align=center|50° (pinholes) |
|||
!width=350 align=center|100° (pinholes) |
|||
!width=350 align=center|250° |
|||
|-align=left |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-50C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 50° Low Stress)]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-100C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 100° Low Stress)]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-250C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 250° Low Stress)]] |
|||
|- |
|||
|} |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe] |
|||
=== SiN (100% SiH<sub>4</sub> ) === |
|||
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] - ''Lists film data, such as dep rate, stress, particle count, refractive index etc.'' |
|||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014] |
|||
|- bgcolor="#D0E7FF" |
|||
!width=350 align=center|50° (pinholes) |
|||
!width=350 align=center|100° (pinholes) |
|||
!width=350 align=center|250° |
|||
|-align=left |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-Low stress SiNx-100%SiH4-120W-50C.pdf|SiN Deposition Recipe (120W 50° Low Stress)]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Deposition Recipe (120W 100° Low Stress)]] |
|||
*[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 120W-100(250)C]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-Low stress SiNx-100% SiH4-120W-250C.pdf|SiN Deposition Recipe (120W 250° Low Stress)]] |
|||
*[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 120W, 100(250)C ]] |
|||
|- align=left |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-Medium stress SiNx-100%SiH4-120W-50C.pdf|SiN Deposition Recipe (50W 50° Medium Stress)]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-Medium stres SiNx-100% SiH4-120W-100C.pdf|SiN Deposition Recipe (50W 100° Medium Stress)]] |
|||
*[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 50W, 100(250)C]] |
|||
*[[Media:27-SiNx_Film_(Bias%3D50W)_Sidewall_Coverage.pdf|SiN SEM sidewall coverage]] |
|||
| |
|||
*[[Media:PECVD2-SiN-Recipe-Medium stress SiNx-100% SiH4-120W-250C.pdf|SiN Deposition Recipe (50W 250° Medium Stress)]] |
|||
*[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN ComparisonTable 50W, 100(250)C]] |
|||
|- |
|||
|} |
|||
==Standard Cleaning Procedure (PECVD #1)== |
|||
==SiO<sub>2</sub> deposition (Unaxis VLR) == |
|||
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. |
|||
=== SiO<sub>2</sub> (2% SiH<sub>4</sub>) === |
|||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
|- bgcolor="#D0E7FF" |
|||
!width=350 align=center|50° |
|||
!width=350 align=center|100° |
|||
!width=350 align=center|250° |
|||
|-align=left |
|||
| |
|||
*[[Media:PECVD2-SiO2Recipe-5W-50C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 50°)]] |
|||
| |
|||
*[[Media:PECVD2-SiO2Recipe-5W-100C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 100°)]] |
|||
*[[Media:SiO2 film Unaxis ICP vs PECVD I.pdf|SiO<sub>2</sub> film Unaxis ICP vs PECVD I]] |
|||
*[[Media:SEM pictures SiO2 100C.pdf|SiO<sub>2</sub> SEM pictures 100C]] |
|||
| |
|||
*[[Media:PECVD2-SiO2Recipe-5W-250C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 250°)]] |
|||
*[[Media:SiO2 film Unaxis ICP vs PECVD I.pdf|SiO<sub>2</sub> film Unaxis ICP vs PECVD I]] |
|||
|- |
|||
|} |
|||
The clean is done in two steps: |
|||
=== SiO<sub>2</sub> (2% SiH<sub>4</sub> - No Ar) === |
|||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
|- bgcolor="#D0E7FF" |
|||
!width=350 align=center|50° |
|||
!width=350 align=center|100° |
|||
!width=350 align=center|250° |
|||
|-align=left |
|||
| |
|||
*[[Media:PECVD2-SiO2-Recipe-NoAr-50C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (50°)]] |
|||
*[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]] |
|||
| |
|||
*[[Media:PECVD2-SiO2-Recipe-NoAr-100C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (100°)]] |
|||
*[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]] |
|||
| |
|||
*[[Media:PECVD2-SiO2-Recipe-NoAr-250C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (250°)]] |
|||
*[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]] |
|||
|- |
|||
|} |
|||
#'''Wet cleaning''' (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. ) |
|||
=== SiO<sub>2</sub> (100% SiH<sub>4</sub> HDR) === |
|||
#Load the recipe for plasma cleaning "'''''CF4/O2 Clean'''''" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning. |
|||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
|- bgcolor="#D0E7FF" |
|||
{| class="wikitable" |
|||
!width=350 align=center|50° |
|||
|+Table of Cleaning Times |
|||
!width=350 align=center|100° |
|||
!Film Dep'd |
|||
!width=350 align=center|250° |
|||
!Cleaning Time |
|||
|-align=left |
|||
| |
|- |
||
|SiO<sub>2</sub> |
|||
*[[Media:SiO2 100% SiH4 HDR 50C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (50°)]] |
|||
|1 min clean for every 1 min dep |
|||
| |
|||
|- |
|||
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-HDR-100C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (100°)]] |
|||
|Si<sub>3</sub>N<sub>4</sub> |
|||
*[[Media:PECVD2-SiO2-HDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - HDR (100°)]] |
|||
|1 min clean for every 7 min dep |
|||
| |
|||
|- |
|||
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-HDR-250C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (250°)]] |
|||
|SiOxNy |
|||
*[[Media:PECVD2-SiO2-HDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - HDR (250°)]] |
|||
|Same as SiO<sub>2</sub> |
|||
|- |
|- |
||
|a-Si |
|||
|Same time as Si<sub>3</sub>N<sub>4</sub> |
|||
|} |
|} |
||
===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]=== |
|||
=== SiO<sub>2</sub> (100% SiH<sub>4</sub> LDR) === |
|||
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that '''it will pop up a window for the cleaning time''' upon running the recipe - you do not need to edit the recipe before running it. |
|||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
|- bgcolor="#D0E7FF" |
|||
!width=350 align=center|50° |
|||
!width=350 align=center|100° |
|||
!width=350 align=center|250° |
|||
|-align=left |
|||
| |
|||
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-50C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (50°)]] |
|||
| |
|||
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-100C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (100°)]] |
|||
*[[Media:PECVD2-SiO2-LDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - LDR (100°)]] |
|||
*[[Media:PECVD2-SiO2-SEM-LDR SiO2-100% SiH4-100C-15W.pdf|SiO<sub>2</sub> SEM sidewall coverage]] |
|||
| |
|||
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-250C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (250°)]] |
|||
*[[Media:PECVD2-SiO2-LDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - LDR (250°)]] |
|||
|- |
|||
|} |
|||
=[[PECVD 2 (Advanced Vacuum)]]= |
|||
=== Amorphous Si (100%SiH<sub>4</sub> Ar He) === |
|||
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
===[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=272916741 PECVD 2 Process Control Plots] - Plots of all process control data=== |
|||
|- bgcolor="#D0E7FF" |
|||
!width=350 align=center|90° |
|||
==SiO<sub>2</sub> deposition (PECVD #2)== |
|||
!width=350 align=center|250° |
|||
|-align=left |
|||
*[https://docs.google.com/spreadsheets/d/1cYK-k669vf8YO2q2YCGa3gTdaDI3I3M-a9KR5RDlZWY/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD SiO2 v2''" |
|||
| |
|||
**[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''STD SiO2''" |
|||
*[[Media:02-ICP-PECVD-a-Si_Film-90C.pdf|a-Si Deposition Recipe - 90°]] |
|||
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=1313651154 SiO<sub>2</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
|||
| |
|||
**Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
*[[Media:01-ICP-PECVD-a-Si-Deposition_Recipe-250C.pdf|a-Si Deposition Recipe - 250°]] |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.232.29 SiO<sub>2</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021 |
|||
*SiO<sub>2</sub> deposition rate at 150C is 35nm/min |
|||
==SiN deposition (PECVD #2)== |
|||
*[https://docs.google.com/spreadsheets/d/1JBXEfRGemFJK81RkHfxS0cTucb3viUL7hMGzmKRD5uU/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD Si3N4 v3''" |
|||
**[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''Nitride2''" |
|||
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=773875841 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
|||
**Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.232.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021 |
|||
==Low-Stress SiN deposition (PECVD #2)== |
|||
''Low-Stress Silicon Nitride, Si<sub>3</sub>N<sub>4</sub> (< ±100 MPa)'' |
|||
*[https://docs.google.com/spreadsheets/d/19VQ6ytYbZ5SsAiXzgWqwlyJUqgjWb8x_eyv7L8DvtwM/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD LS-Si3N4 v4''" |
|||
**[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "'' Old LSNitride2 recipe ''" |
|||
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
|||
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=203400760 Plots of Low-Stress Si<sub>3</sub>N<sub>4</sub> Process Control Data] |
|||
**Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
*[[Old Deposition Data - 2021-12-15#Low-Stress SiN deposition .28PECVD .232.29|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data - Before Oct. 2021</nowiki>]] |
|||
*:''Old Versions of the recipe:'' |
|||
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]'' |
|||
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018]'' |
|||
===Low-Stress SiN 3xTime (PECVD #2)=== |
|||
''This Low-Stress SiN recipe is more stable over time (months), because each step is 3x longer (so each compressive/tensile layer is thicker), making it less susceptible to RF ignition delays as the grounding strap is etched over time. – 2024-09 [[Demis D. John|Demis]] & [[Biljana Stamenic|Biljana]]'' |
|||
*Recipe: "''[https://docs.google.com/spreadsheets/d/1OQp_sux5YEgpcyH3sf0JCwTOhvoi_LSYKOUMRR4Umh4?usp=drive_fs STD LS-Si3N4 3xTime v1]"'' |
|||
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?usp=sharing Process Control Data]: Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?gid=974005628#gid=974005628 Process Control Charts/Plots]: Calibration control limits versus date |
|||
==Amorphous-Si deposition (PECVD #2)== |
|||
*[[PECVD-2 - a-Si Recipe and Dep process (2025)|a-Si Recipe and Dep process]] 2025-11 |
|||
**''Developed by Ryan Hersey & Skyler Palatnik, Group of Prof. Max Millar-Blanchaer'' |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe] (2013-09, Ning Cao) |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Film - Characterization and Stress] - DOE/recipe variations |
|||
==Standard Cleaning Procedure (PECVD #2)== |
|||
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps: |
|||
#If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head! |
|||
#Load the recipe for cleaning "STD CF<sub>4</sub>/O<sub>2</sub> Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning. |
|||
===[https://wiki.nanofab.ucsb.edu/wiki/File:STD_CF4-O2_Clean_PECVD2.jpg Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"]=== |
|||
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it. |
|||
'''Clean Times (PECVD#2''') |
|||
{| class="wikitable" |
|||
!Film Deposited |
|||
!Cleaning Time (Dry) |
|||
|- |
|- |
||
|SiO<sub>2</sub> |
|||
|1min. clean for every 1min. deposition |
|||
|- |
|||
|Si<sub>3</sub>N<sub>4</sub> |
|||
|1min. clean for every 7min. of deposition |
|||
|- |
|||
|a-Si |
|||
|2 min clean for every 1min of deposition |
|||
|- |
|||
|a-Si (max 60min dep before breaking it up and cleaning the chamber) |
|||
|Wet Clean the Upper Lid/Chamber |
|||
DI water then Isopropyl Alcohol on chamber wall & portholes |
|||
|- |
|||
|Other films:(max 60min long dep. in one single run) |
|||
|If > 29min total dep time |
|||
(Season + Dep) |
|||
Wet Clean the Upper Lid/Chamber |
|||
DI water then Isopropyl Alcohol on chamber wall & portholes |
|||
|} |
|} |
||
=[[ICP-PECVD (Unaxis VLR)]]= |
|||
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the [[ICP-PECVD (Unaxis VLR)#Documentation|new procedures]] to ensure low particle counts in the chamber. |
|||
The system currently has '''Deuterated Silane (SiD<sub>4</sub>)''' installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films. |
|||
==Process Control Data (Unaxis ICP-PECVD)== |
|||
''Regularly-run depositions and measurements of film properties over time - executed by [https://nanofab.ucsb.edu/workforce NanoFab Interns].'' |
|||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Process Control Plots] - ''Plots of all Process Control data'' |
|||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub>] |
|||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub>] |
|||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub>] |
|||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub>] |
|||
==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]== |
|||
*[https://docs.google.com/spreadsheets/d/1mobnAIH70a9eFbCkMnza2WfpI2uRUWtLlz0cLK1Ljuo/edit?gid=1554182668#gid=1554182668 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C-new May 2024'' |
|||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Process Control Data</nowiki>] |
|||
**Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
=== Old Data === |
|||
* [https://docs.google.com/spreadsheets/d/17ft9jrHcCFCp2830RsLwQq5lHuupWATXT91SreG8WYY/edit#gid=143856038 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C - replaced on May 2024''" |
|||
* [https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=1199123007 Old Recipe] - 2019 |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_LDR_250C_Deposition_.28Unaxis_VLR.29 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021 |
|||
==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]== |
|||
*[https://docs.google.com/spreadsheets/d/1x0mB4ySSUfEAfRehAx7k_k3BJuTMczaRxQgxsTAFfo4/edit?gid=744785272#gid=744785272 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-new May 2024''" |
|||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>] |
|||
**Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
=== Old Data === |
|||
*[https://docs.google.com/spreadsheets/d/13KUlUujEWSLOH54Ibd52YNJPZcAc7ELShI2RAqM6H-Y/edit#gid=117484667 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-replace on May 2024''" |
|||
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=1199123007 Old Recipe] - 2019 |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_HDR_250C_Deposition_.28Unaxis_VLR.29 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] |
|||
==Gap-Fill SiO<sub>2</sub> [ICP-PECVD]== |
|||
''Recipe designed by [https://scholar.google.com/citations?user=kur3-cEAAAAJ&hl=en&oi=ao Warren Jin], please consider our [https://wiki.nanotech.ucsb.edu/wiki/Frequently_Asked_Questions#Publications_acknowledging_the_Nanofab publication policy] if you publish using this recipe.'' |
|||
'''NOTE:''' Please contact tool [[Tony Bosch|supervisor]] before running this recipe - this recipe must often be scheduled to prevent excessive chamber maintenance. |
|||
Able to effectively fill ~1:1 and ~1:2 aspect ratio gaps in Silicon and Glass structures (eg. waveguides/optical gratings) with void-free filling. |
|||
The recipe uses a high 400W RF Bias to reduce buildup on corners that causes voids during growth. |
|||
*Category = <code>SiO2 GapFill - Std.</code> |
|||
*FLOW: <code>SiO2 GapFill 250C</code> |
|||
**Will run the sequence <code>SiO2 GapFill 250C 450W</code>. Do not change this! |
|||
*STEP (edit TIME only): <code>SiO2 GapFill 250C</code> |
|||
*Deposition rate = 99.968nm/min [9/20/23] |
|||
==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
|||
*[https://docs.google.com/spreadsheets/d/18nE-iTLLH4QIq3wadHVgjVuZ215o9xUz_aCX2WDdges/edit?gid=638997025#gid=638997025 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C-new May 2024''" |
|||
* [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>] |
|||
** Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
=== Old Data === |
|||
*[https://docs.google.com/spreadsheets/d/1Np5uJ1bw81MxHlDD0qs5Jh_hj7nCSznQTsSEELlT414/edit?usp=sharing Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C- replaced on May 2024''" |
|||
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Old Recipe] - 2019 |
|||
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_250C_deposition_.28Unaxis_VLR.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021 |
|||
==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
|||
*[https://docs.google.com/spreadsheets/d/1xchMuXlPABSKcW-rMau8B-cw_jnJnwI9qpXqDLUQ8sU/edit?gid=1239658204#gid=1239658204 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C-new May 2024''" |
|||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>] |
|||
**Lists film data, such as dep rate, stress, particle count, refractive index etc. |
|||
=== Old Data === |
|||
* [https://docs.google.com/spreadsheets/d/1JuQlCU-mozIUJx9z9aQdisIJyFhv1r9AWI8EWeOnsPo/edit#gid=82816489 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C - replaced on May 2024''" |
|||
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Old Recipe] - 2019 |
|||
==Standard Seasoning Procedure [ICP-PECVD]== |
|||
You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film]. |
|||
Seasoning recipes: |
|||
*[https://docs.google.com/spreadsheets/d/1S01xgtxFEJ4q7GLHfo-96yYKxer8nGlB/edit?gid=1944526099#gid=1944526099 SiO<sub>2</sub> seasoning - Std ] |
|||
*[https://docs.google.com/spreadsheets/d/1S3BFJIn9oAq2bxg6PDe9RY_6Fvkc36ki/edit?gid=1218243940#gid=1218243940 SiN seasoning - Std ] |
|||
==Standard Cleaning Procedure [ICP-PECVD]== |
|||
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details. |
|||
*SiNx etches at 20nm/min |
|||
*SiO<sub>2</sub> etches at 40nm/min |
|||
===Standard Clean Recipe=== |
|||
*[https://docs.google.com/spreadsheets/d/1S3DzvJJahNTwGXsn0GDyg2FiourGffiy/edit?gid=2021404224#gid=2021404224 Post Deposition Clean 250C ] |
|||
==General Recipe Notes (Unaxis VLR ICP-PECVD)== |
|||
*RF1 = Bias |
|||
*RF2 = ICP Power |
|||
*All recipes start with an Argon pre-clean with 0W bias (gentle), to improve adhesion/nucleation. |
|||
*Maximum SiO<sub>2</sub> Dep. thickness allowed: 800nm |
|||
**Above this thickness, you must run a chamber clean/season before depositing more onto your product wafer. |
|||
Latest revision as of 18:07, 10 December 2025
Back to Vacuum Deposition Recipes.
PECVD 1 (PlasmaTherm 790)
PECVD 1 Process Control Plots - Plots of all process control data
SiO2 deposition (PECVD #1)
- SiO2 [PECVD 1] Current Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
Old Data
- SiO2 [PECVD 1] Historical Data - Oct. 2021 and earlier
SiN deposition (PECVD #1)
- Si3N4 [PECVD 1] Standard Recipe
- Si3N4 [PECVD 1] Current Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
Old Data
- Si3N4 [PECVD 1] Historical Data - Oct. 2021 and earlier
Low Stress Si3N4 (PECVD#1)
- Low Stress Si3N4 [PECVD 1] Standard Recipe
- Low Stress Si3N4 [PECVD 1] Historical Data - 2021-10 and earlier

Example of Si3N4 modified stress via. varying N2 flow. Refractive index is relatively constant (one outlier), and stress varies continuously from tensile to compressive. (Demis D. John 2011, Blumenthal Group)
SiOxNy deposition (PECVD #1)
- SiOxNy Standard Recipe
- SiOxNy Data 2014 - Lists film data, such as dep rate, stress, particle count, refractive index etc.
- SiOxNy1000A Thickness uniformity 2014
Standard Cleaning Procedure (PECVD #1)
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.
The clean is done in two steps:
- Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
- Load the recipe for plasma cleaning "CF4/O2 Clean" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.
| Film Dep'd | Cleaning Time |
|---|---|
| SiO2 | 1 min clean for every 1 min dep |
| Si3N4 | 1 min clean for every 7 min dep |
| SiOxNy | Same as SiO2 |
| a-Si | Same time as Si3N4 |
Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
PECVD 2 (Advanced Vacuum)
PECVD 2 Process Control Plots - Plots of all process control data
SiO2 deposition (PECVD #2)
- SiO2 [PECVD 2] New Standard Recipe - "STD SiO2 v2"
- SiO2 [PECVD 2] Old Standard Recipe - "STD SiO2"
- SiO2 [PECVD 2] Current Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
- SiO2 [PECVD 2] Historical Data - Before Oct. 2021
- SiO2 deposition rate at 150C is 35nm/min
SiN deposition (PECVD #2)
- Si3N4 [PECVD 2] New Standard Recipe - "STD Si3N4 v3"
- Si3N4 [PECVD 2] Old Standard Recipe - "Nitride2"
- Si3N4 [PECVD 2] Current Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
- Si3N4 [PECVD 2] Historical Data - Before Oct. 2021
Low-Stress SiN deposition (PECVD #2)
Low-Stress Silicon Nitride, Si3N4 (< ±100 MPa)
- Low Stress Si3N4 [PECVD 2] New Standard Recipe - "STD LS-Si3N4 v4"
- Low Stress Si3N4 [PECVD 2] Old Standard Recipe - " Old LSNitride2 recipe "
- Low Stress Si3N4 [PECVD 2] Current Process Control Data
- Plots of Low-Stress Si3N4 Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
- Low Stress Si3N4 [PECVD 2] Historical Data - Before Oct. 2021
- Old Versions of the recipe:
- LS Nitride2 Standard Recipe 2014-5/9/2018
- STD LSNitride2 5/9/2018
Low-Stress SiN 3xTime (PECVD #2)
This Low-Stress SiN recipe is more stable over time (months), because each step is 3x longer (so each compressive/tensile layer is thicker), making it less susceptible to RF ignition delays as the grounding strap is etched over time. – 2024-09 Demis & Biljana
- Recipe: "STD LS-Si3N4 3xTime v1"
- Process Control Data: Lists film data, such as dep rate, stress, particle count, refractive index etc.
- Process Control Charts/Plots: Calibration control limits versus date
Amorphous-Si deposition (PECVD #2)
- a-Si Recipe and Dep process 2025-11
- Developed by Ryan Hersey & Skyler Palatnik, Group of Prof. Max Millar-Blanchaer
- Amorphous Si Deposition Recipe (2013-09, Ning Cao)
- Amorphous Si Film - Characterization and Stress - DOE/recipe variations
Standard Cleaning Procedure (PECVD #2)
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
- If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
- Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.
Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
Clean Times (PECVD#2)
| Film Deposited | Cleaning Time (Dry) |
|---|---|
| SiO2 | 1min. clean for every 1min. deposition |
| Si3N4 | 1min. clean for every 7min. of deposition |
| a-Si | 2 min clean for every 1min of deposition |
| a-Si (max 60min dep before breaking it up and cleaning the chamber) | Wet Clean the Upper Lid/Chamber
DI water then Isopropyl Alcohol on chamber wall & portholes |
| Other films:(max 60min long dep. in one single run) | If > 29min total dep time
(Season + Dep) Wet Clean the Upper Lid/Chamber DI water then Isopropyl Alcohol on chamber wall & portholes |
ICP-PECVD (Unaxis VLR)
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.
Process Control Data (Unaxis ICP-PECVD)
Regularly-run depositions and measurements of film properties over time - executed by NanoFab Interns.
- ICP-PECVD Process Control Plots - Plots of all Process Control data
- Low Deposition Rate SiO2
- High Deposition Rate SiO2
- Si3N4
- Low Stress Si3N4
Low Deposition Rate SiO2 [ICP-PECVD]
- Low Deposition Rate SiO2 [ICP-PECVD] - Standard Recipe - "SiO2 LDR250C-new May 2024
- Low Deposition Rate SiO2 [ICP-PECVD] - Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
Old Data
- Low Deposition Rate SiO2 [ICP-PECVD] - Standard Recipe - "SiO2 LDR250C - replaced on May 2024"
- Old Recipe - 2019
- Low Deposition Rate SiO2 [ICP-PECVD] - Historical Data - before Oct. 2021
High Deposition Rate SiO2 [ICP-PECVD]
- High Deposition Rate SiO2 [ICP-PECVD] - Standard Recipe - "SiO2 HDR250C-new May 2024"
- High Deposition Rate SiO2 [ICP-PECVD] - Current Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
Old Data
- High Deposition Rate SiO2 [ICP-PECVD] - Standard Recipe - "SiO2 HDR250C-replace on May 2024"
- Old Recipe - 2019
- High Deposition Rate SiO2 [ICP-PECVD] - Historical Data
Gap-Fill SiO2 [ICP-PECVD]
Recipe designed by Warren Jin, please consider our publication policy if you publish using this recipe.
NOTE: Please contact tool supervisor before running this recipe - this recipe must often be scheduled to prevent excessive chamber maintenance.
Able to effectively fill ~1:1 and ~1:2 aspect ratio gaps in Silicon and Glass structures (eg. waveguides/optical gratings) with void-free filling.
The recipe uses a high 400W RF Bias to reduce buildup on corners that causes voids during growth.
- Category =
SiO2 GapFill - Std. - FLOW:
SiO2 GapFill 250C- Will run the sequence
SiO2 GapFill 250C 450W. Do not change this!
- Will run the sequence
- STEP (edit TIME only):
SiO2 GapFill 250C - Deposition rate = 99.968nm/min [9/20/23]
Si3N4 [ICP-PECVD]
- Si3N4 [ICP-PECVD] - Standard Recipe - "SiN 250C-new May 2024"
- Si3N4 [ICP-PECVD] - Current Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
Old Data
- Si3N4 [ICP-PECVD] - Standard Recipe - "SiN 250C- replaced on May 2024"
- Old Recipe - 2019
- Si3N4 [ICP-PECVD] - Historical Data - before Oct. 2021
Low Stress Si3N4 [ICP-PECVD]
- Low Stress Si3N4 [ICP-PECVD] - Standard Recipe - "SiN Low Stress 250C-new May 2024"
- Low Stress Si3N4 [ICP-PECVD] - Current Process Control Data
- Lists film data, such as dep rate, stress, particle count, refractive index etc.
Old Data
- Low Stress Si3N4 [ICP-PECVD] - Standard Recipe - "SiN Low Stress 250C - replaced on May 2024"
- Old Recipe - 2019
Standard Seasoning Procedure [ICP-PECVD]
You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film]. Seasoning recipes:
Standard Cleaning Procedure [ICP-PECVD]
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.
- SiNx etches at 20nm/min
- SiO2 etches at 40nm/min
Standard Clean Recipe
General Recipe Notes (Unaxis VLR ICP-PECVD)
- RF1 = Bias
- RF2 = ICP Power
- All recipes start with an Argon pre-clean with 0W bias (gentle), to improve adhesion/nucleation.
- Maximum SiO2 Dep. thickness allowed: 800nm
- Above this thickness, you must run a chamber clean/season before depositing more onto your product wafer.