Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean": cleaning procedure after a-Si dep
 
(428 intermediate revisions by 4 users not shown)
Line 1: Line 1:
{{recipes|Vacuum Deposition}}
{{recipes|Vacuum Deposition}}

=[[PECVD 1 (PlasmaTherm 790)]]=
=[[PECVD 1 (PlasmaTherm 790)]]=
Note: Software upgrade performed on 2018-10-10. Note any changes in film.
*[https://docs.google.com/spreadsheets/d/1a0XrY6HuJ6L9niThZYI-u4XH69Hnbe3jkm1qKmrR8Rg/edit#gid=sharing Particulates (Gain4) in PECVD#1 2015]
*[https://docs.google.com/spreadsheets/d/1ZfkspbCQZmdThC8qB4XyjsyPAzrMF1QbHSMFmH6xSo4/edit#gid=sharing Particulates (Gain4) in PECVD#1 2016]
*[https://docs.google.com/spreadsheets/d/1YNiof68Veeh08s_NtG5aCWUXW7GWDDU00HAimV_l8_g/edit#gid=sharing Particulates (Gain4) in PECVD#1 2017]


===[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1270764394 PECVD 1 Process Control Plots] - Plots of all process control data===


==SiO<sub>2</sub> deposition (PECVD #1)==
*[https://docs.google.com/spreadsheets/d/1VN551M2oXGWX306HDLQXvZIp3kgxEvWffQqMqnc8ISk/edit#gid=sharing Particulates in PECVD#1 films 2017]
*[https://docs.google.com/spreadsheets/d/11c0gQHnattIjVO95aBqiL-zL4DInRFihV-YB54xLT40/edit#gid=sharing Particulates in PECVD1 films 2018]
== SiN deposition (PECVD #1) ==
*[[media:New PECVD1-SiO2-standard recipe 2014 SiO2 standard recipe.pdf|SiN Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN 100nm Data 2014]
*[https://docs.google.com/spreadsheets/d/1phx1WficlUEg0xSahaAq4zrRk6m9Eb0ausO8wcAmXqs/edit#gid=sharing SiN 100nm Data 2015]
*[https://docs.google.com/spreadsheets/d/1VNSNTqnbE4SFk0HyhBAy3GJzi0jRQEs8cgk1v2_Uam8/edit#gid=sharing SiN 100nm Data 2016]
*[https://docs.google.com/spreadsheets/d/1TG1X2wpl2fWaHEtAHtpZFBVSCk1BQeGJQ8LA2M2qBJ0/edit#gid=sharing SiN 100nm Data 2017]
*[https://docs.google.com/spreadsheets/d/1UlyvPcXUBQ5R2JwjKOjELvtCJaTElVhJHfzgjyaRd2A/edit#gid=sharing SiN 300nm Data 2017]
*[https://docs.google.com/spreadsheets/d/1pAoTCaNSf0uZMyiQ2qKFd0s_e4e53P9Z1jUwtmTnlLk/edit#gid=sharing SiN 300nm Data 2018]


*[https://docs.google.com/spreadsheets/d/1wloq6HJw5RQIvmeKcBn3xvE_917R6jF_K-btCHjsiIM/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]


*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 100 nm Thickness uniformity 2014]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://docs.google.com/spreadsheets/d/1-pET1Eojooso5UHk90W-5uYByDDdrCyRnggqewxTmVg/edit#gid=sharing SiN 100 nm Thickness uniformity 2015]
*[https://docs.google.com/spreadsheets/d/1V_-KzsdR-2tSnJGtUdQWokmnNIY949t0vdQOp7RfCgc/edit#gid=sharing SiN 100 nm Thickness uniformity 2016]
*[https://docs.google.com/spreadsheets/d/1tM-a4VBEqpxr2G8PGGLTbsR6BQBmvqXNRBw0mikAUS0/edit#gid=sharing SiN 100 nm Thickness uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1Z83RCH5cAUfViO6vv6hAatcLVWZ95ex4nDdfffm9I7s/edit#gid=sharing SiN 300nm Thickness uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1b4EQZdRtVbqNwGBrItoG5-tz6RIzlsvBiCFR6ZXfylw/edit#gid=sharing SiN 300nm Thickness uniformity 2018]


=== Old Data ===
== SiO<sub>2</sub> deposition (PECVD #1) ==
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.231.29 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier
*[[media:New PECVD1-SiN-standard recipe 2014 SiN standard recipe.pdf|SiO<sub>2</sub> Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEw0bjFEdTF2SUhRa25Ca0d0SzBha3c&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Data 2014]
*[https://docs.google.com/spreadsheets/d/1JWNUcH8l90xif-0BhYKJee9nXxE4hnvvp6N2NtZLYXY/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2015]
*[https://docs.google.com/spreadsheets/d/1F2pfsVnbUgaE9tsm8HZMlY6cyt-nhui0IpvGc6udhDU/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2016]
*[https://docs.google.com/spreadsheets/d/1MblK5Zr5Skfw0s9Hdhqr_cCwN-nCgM-ofZnsAyvVRq8/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2017]
*[https://docs.google.com/spreadsheets/d/15SocIqWQvBKSvT5oCWoZAURLaaqb9KosxCN2rueZQN8/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2017]
*[https://docs.google.com/spreadsheets/d/1DdjIRGsfJ7WCrxQoGpmzkjLGJhpBTFNYLFmmHcNjAjk/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2018]


==SiN deposition (PECVD #1)==


*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=98787450 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.


=== Old Data ===
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDQ3VEtZQVRpdVdlbGtIZHpTNmFzNmc&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Thickness uniformity 2014]
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.231.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier
*[https://docs.google.com/spreadsheets/d/1NQy-ADou6f2NBU-9jZG8KME1lOz0X5mh6HZV9_jPGes/edit#gid=sharing SiO<sub>2</sub> 100 nm Thickness uniformity 2015]
*[https://docs.google.com/spreadsheets/d/1WUCm_dWpxKTjfFf1rNfLuxvwMxsyCYON_OZ3gb50L_s/edit#gid=sharing SiO<sub>2</sub> 100 nmThickness uniformity 2016]
*[https://docs.google.com/spreadsheets/d/1dpC_AkPD-etIH6fVuQqLfd4UMNQCEtcqhvmBpwbEncE/edit#gid=sharing SiO<sub>2</sub> 100nm Thickness uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1Fa8mZIBIeJwvCwUbJ-28VcvVYj8rshhuDuXsYxA-cD8/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1YB_9USpuXGpIdSW2gNsptu5nSrLWAGsYu0SWoYEy0aQ/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2018]


== OTHER recipes: Low-Stress (LS) SiN and SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1) ==
==Low Stress Si<sub>3</sub>N<sub>4</sub> (PECVD#1)==

<!-- Placeholders - Not uploaded yet-->
*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
*[[media:New PECVD1-LS SIN-Turner05recipe 2014 LS SIN recipe.pdf|LS SiN Standard Recipe]]
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#Low-Stress_SiN_-_LS-SiN_.28PECVD.231.29 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - 2021-10 and earlier
*[https://docs.google.com/spreadsheets/d/1Joz0az9TGZWQc4CiMQJZzLBbNFbx_hH2Oc0B4NNJmYk/edit#gid=sharing LS SiN Data 2014]

*[https://docs.google.com/spreadsheets/d/1xIzc2CufRYNSfAtsOXpw3IzHreeu42BWrLBV0kzP6kA/edit#gid=sharing LS SiN 1000A Thickness uniformity 2014]
:[[File:PECVD1 SiN Stress vs. N2 plot.jpg|alt=plot of SiN stress and Refractive Index vs. N2 flow. |none|thumb|414x414px|Example of Si<sub>3</sub>N<sub>4</sub> modified stress via. varying N<sub>2</sub> flow.  Refractive index is relatively constant (one outlier), and stress varies continuously from tensile to compressive.  ([[Demis D. John]] 2011, [https://engineering.ucsb.edu/people/daniel-blumenthal Blumenthal Group])]]
*[[media:New PECVD1-LS SION-recipe 2014 LS SION recipe.pdf|SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]]

*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014]
==SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1)==

*[https://wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] - ''Lists film data, such as dep rate, stress, particle count, refractive index etc.''
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]

==Standard Cleaning Procedure (PECVD #1)==
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.

The clean is done in two steps:

#'''Wet cleaning''' (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
#Load the recipe for plasma cleaning "'''''CF4/O2 Clean'''''" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.

{| class="wikitable"
|+Table of Cleaning Times
!Film Dep'd
!Cleaning Time
|-
|SiO<sub>2</sub>
|1 min clean for every 1 min dep
|-
|Si<sub>3</sub>N<sub>4</sub>
|1 min clean for every 7 min dep
|-
|SiOxNy
|Same as SiO<sub>2</sub>
|-
|a-Si
|Same time as Si<sub>3</sub>N<sub>4</sub>
|}

===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]===
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that '''it will pop up a window for the cleaning time''' upon running the recipe - you do not need to edit the recipe before running it.


=[[PECVD 2 (Advanced Vacuum)]]=
=[[PECVD 2 (Advanced Vacuum)]]=
*[https://docs.google.com/spreadsheets/d/1kj0SWxRpnPRoGld8k3sW-3yK1iPm3buTkvlJSN5YPV4/edit#gid=sharing Particulates (Gain4) in PECVD#2 2015]
*[https://docs.google.com/spreadsheets/d/1xpk9tJrE68NIJ_1yIym0xBxd4fnzHHBHdkhFehruO3E/edit#gid=sharing Particulates (Gain4) in PECVD#2 2016]
*[https://docs.google.com/spreadsheets/d/1ICgt-fgTvNPbE_65x5jUsqy8JjHVv5WUvmE7g7VUbsI/edit#gid=sharing Particulates (Gain4) in PECVD#2 2017]


*[https://docs.google.com/spreadsheets/d/1yPAPP24z3RcRRi-HqEp3GJN4JM8Ec8SFJwZ-OYGG2HU/edit#gid=sharing Particulates in PECVD#2 films 2017]
===[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=272916741 PECVD 2 Process Control Plots] - Plots of all process control data===
*[https://docs.google.com/spreadsheets/d/1aU6fTyQ5MlGD4uCa9gepG5rLJzW3wlkOWSKEl_w_Ye4/edit#gid=sharing Particulates in PECVD#2 films 2018]
== SiO<sub>2</sub> deposition (PECVD #2) ==
*[[media:New Adv PECVD OXIDE 300C standard recipe OXIDE Standard Recipe.pdf|Oxide Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]
*[https://docs.google.com/spreadsheets/d/1d5boeJRWWgMqvQe6nVM7m8s3KAcS4Yp2L5CEU9svkX4/edit#gid=sharing Oxide Data 2015]
*[https://docs.google.com/spreadsheets/d/1XQRcTJdw9AIMPAUsH0n9Ic9Fe1_xGDSvAxD4gVc9FBw/edit#gid=sharing Oxide data 2016]
*[https://docs.google.com/spreadsheets/d/1vcaHwraMGNHuRxgWwGp78EJf4T3Jk182wxoCz_neuck/edit#gid=sharing Oxide Data 2017]
*[https://docs.google.com/spreadsheets/d/1VI-sUmaqois0NsCvf2kQmPfRRa03MjBzl779hmmLtP4/edit#gid=sharing Oxide Data 2018]


==SiO<sub>2</sub> deposition (PECVD #2)==


*[https://docs.google.com/spreadsheets/d/1cYK-k669vf8YO2q2YCGa3gTdaDI3I3M-a9KR5RDlZWY/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD SiO2 v2''"
**[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''STD SiO2''"
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=1313651154 SiO<sub>2</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.232.29 SiO<sub>2</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021


*SiO<sub>2</sub> deposition rate at 150C is 35nm/min
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness Uniformity 2014]
*[https://docs.google.com/spreadsheets/d/16pZHcGwesXB1mMPwntOudBIlPvRh6A6DI37DEwyYfPw/edit#gid=sharing Oxide Thickness Uniformity 2015]
*[https://docs.google.com/spreadsheets/d/10OEuANVNmHqWvx-92zibechIrHK5kgqSK4B_O_O3-YI/edit#gid=sharing Oxide Thickness Uniformity 2016]
*[https://docs.google.com/spreadsheets/d/19JjJYdFNFzO685Hp9hODVRFAYF5bP3IEYGTRGQjqLN4/edit#gid=sharing Oxide Thickness Uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2018]


== SiN deposition (PECVD #2) ==
==SiN deposition (PECVD #2)==
*[[media:New Adv PECVD-Nitride2 300C standard recipe Nitride2 Standard Recipe.pdf|Nitride2 Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]
*[https://docs.google.com/spreadsheets/d/1SkYqOwgjUyMaFBPhuTjMvBTXu0KdQFNmITryF_OVi8o/edit#gid=sharing Nitride2 Data 2015]
*[https://docs.google.com/spreadsheets/d/1HJszgZyEZR9ZsiJpQM6pdsoQ6pWwI6brXasdmfDRoBQ/edit#gid=sharing Nitride2 Data 2016]
*[https://docs.google.com/spreadsheets/d/1f3JBEnr7lf0yIMlzlOYKv_bXlIDyXt8vec_rSVJIoOk/edit#gid=sharing Nitride2 Data 2017]
*[https://docs.google.com/spreadsheets/d/1OO0ewGSqYSzL3lj8fXkgckTkBGQRliD6sBc02IW7wZY/edit#gid=sharing Nitride2 Data 2018]


*[https://docs.google.com/spreadsheets/d/1JBXEfRGemFJK81RkHfxS0cTucb3viUL7hMGzmKRD5uU/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD Si3N4 v3''"
**[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''Nitride2''"
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=773875841 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.232.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021


==Low-Stress SiN deposition (PECVD #2)==
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness Uniformity 2014]
''Low-Stress Silicon Nitride, Si<sub>3</sub>N<sub>4</sub> (< ±100 MPa)''
*[https://docs.google.com/spreadsheets/d/14_dYQu3z31fF_oxsUUX8BmDucgv6B07xB3_zqP0HmvM/edit#gid=sharing Nitride2 Thickness Uniformity 2015]
*[https://docs.google.com/spreadsheets/d/1qBHs7uALM2OdE-yXOq4uZk6aUQEjZRjG1C6RcMEf0sk/edit#gid=sharing Nitride2 Thickness Uniformity 2016]
*[https://docs.google.com/spreadsheets/d/1WJcYzHUjLrWpys_i-Q96FN_lBDBufpXZKZVEX_gri_Q/edit#gid=sharing Nitride2 Thickness Uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2018]
*[[media:SiNx Films by PECVD2.pdf|SiNx Film Stress vs LF and HF Duration Time, and Gas Flowing-rate]]


*[https://docs.google.com/spreadsheets/d/19VQ6ytYbZ5SsAiXzgWqwlyJUqgjWb8x_eyv7L8DvtwM/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD LS-Si3N4 v4''"
==Low-Stress SiN deposition (PECVD #2) ==
Low-Stress SilIcon Nitride (< 100 MPa)
*[[media:New AdvPECVD-LS Nitride2 300C standard recipe LS Nitride2 standard recipe.pdf| Initial LS Nitride2 Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]
*[https://docs.google.com/spreadsheets/d/16Q6BrPoNiFP0elVoSGwXRfQdHXzAXOgiyqKmEw-4kII/edit#gid=sharing LS Nitride2 Data 2015]
*[https://docs.google.com/spreadsheets/d/1GZ58eFzD-T8DJ2Nsaj74u6cvawzsOI2DmMit6Z7vqys/edit#gid=sharing LS Nitride2 Data 2016]
*[https://docs.google.com/spreadsheets/d/1gGIWqkCnykPgBc3prhXExT7QcNjWm2HdbTtwugNqm18/edit#gid=sharing LS Nitride2 Data 2017]
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS Nitride Data 2018]
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS Nitride Data 2019]


**[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "'' Old LSNitride2 recipe ''"


*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness Uniformity 2014]
*[https://docs.google.com/spreadsheets/d/1LpkaOpr7oNoyvxFkineD7i9FspO6LweJMulvZHJM5Zc/edit#gid=sharing LS Nitride2 Thickness Uniformity 2015]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=203400760 Plots of Low-Stress Si<sub>3</sub>N<sub>4</sub> Process Control Data]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://docs.google.com/spreadsheets/d/1FRzW9BaIPF2D3cxPgjLq8hbvrBHXDNkiW6DiPVKQBRM/edit#gid=sharing LS Nitride2 Thickness Uniformity 2016]
*[[Old Deposition Data - 2021-12-15#Low-Stress SiN deposition .28PECVD .232.29|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data - Before Oct. 2021</nowiki>]]
*[https://docs.google.com/spreadsheets/d/1vyrgvdEZFgnQUilpa5Ka2nOfowY8zlmJfbQ77EamNBg/edit#gid=sharing LS Nitride2 Thickness Uniformity 2017]
*:''Old Versions of the recipe:''
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2018]
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]''
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018]''


===Low-Stress SiN 3xTime (PECVD #2)===
''This Low-Stress SiN recipe is more stable over time (months), because each step is 3x longer (so each compressive/tensile layer is thicker), making it less susceptible to RF ignition delays as the grounding strap is etched over time. – 2024-09 [[Demis D. John|Demis]] & [[Biljana Stamenic|Biljana]]''


*Recipe: "''[https://docs.google.com/spreadsheets/d/1OQp_sux5YEgpcyH3sf0JCwTOhvoi_LSYKOUMRR4Umh4?usp=drive_fs STD LS-Si3N4 3xTime v1]"''
*[[media:STD LSNitride2 12-14-18 recipe.pdf|STD LSNitride2 12/14/2018]]
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?usp=sharing Process Control Data]: Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?gid=974005628#gid=974005628 Process Control Charts/Plots]: Calibration control limits versus date


== Amorphous-Si deposition (PECVD #2) ==
==Amorphous-Si deposition (PECVD #2)==
*[[media:03-Amorphous-Si-PECVD-2.pdf|Amorphous Si Deposition Recipe]]
*[[media:ASi deposition and film stress using AV dep tool.pdf|Amorphous Si Films and Their Stress]]


*[[PECVD-2 - a-Si Recipe and Dep process (2025)|a-Si Recipe and Dep process]] 2025-11
= [[ICP-PECVD (Unaxis VLR)]] =
**''Developed by Ryan Hersey & Skyler Palatnik, Group of Prof. Max Millar-Blanchaer''
==SiN deposition (Unaxis VLR) ==
*[https://wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe] (2013-09, Ning Cao)
=== SiN (2% SiH<sub>4</sub>) ===
*[https://wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Film - Characterization and Stress] - DOE/recipe variations
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#D0E7FF"
! width="350" align="center" |50° (pinholes)
! width="350" align="center" |100° (pinholes)
! width="350" align="center" |250°
|- align="left"
|
*[[Media:PECVD2-SiN-Recipe-5W-50C-High-Stress.pdf|SiN Deposition Recipe (5W 50° High Stress)]]
*[[Media:PECVD2-SiN-Recipe-50W-50C-Medium-Stress.pdf|SiN Deposition Recipe (50W 50° Medium Stress)]]
*[[Media:PECVD2-SiN-Recipe-120W-50C-Low-Stress.pdf|SiN Deposition Recipe (120W 50° Low Stress)]]
|
*[[Media:PECVD2-SiN-Recipe-5W-100C-High-Stress.pdf|SiN Deposition Recipe (5W 100° High Stress)]]
*[[Media:PECVD2-SiN-Recipe-50W-100C-Medium-Stress.pdf|SiN Deposition Recipe (50W 100° Medium Stress)]]
*[[Media:PECVD2-SiN-Recipe-120W-100C-Low-Stress.pdf|SiN Deposition Recipe (120W 100° Low Stress)]]
*[[Media:PECVD2-SiNx-l.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (120W 100° Low Stress)]]
*[[Media:PECVD2-SiNx-medium-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (50W 100° Medium Stress)]]
*[[Media:PECVD2-SiNx -h.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (5W 100° High Stress)]]
*[[Media:PECVD2-SiNx-medium stress-SEM-2% SiH4-100C-50W.pdf|SiNx SEM images (50W 100° Medium Stress)]]
*[[Media:PECVD2-SiNx-high stress-SEM-2% SiH4-100C-5W.pdf|SiNx SEM images (5W 100° High Stress)]]
|
*[[Media:PECVD2-SiN-Recipe-5W-250C-High-Stress.pdf|SiN Deposition Recipe (5W 250° High Stress)]]
*[[Media:PECVD2-SiN-Recipe-50W-250C-Medium-Stress.pdf|SiN Deposition Recipe (50W 250° Medium Stress)]]
*[[Media:PECVD2-SiN-Recipe-120W-250C-Low-Stress.pdf|SiN Deposition Recipe (120W 250° Low Stress)]]
*[[Media:PECVD2-SiNx-l.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (120W 250° Low Stress)]]
*[[Media:PECVD2-SiNx-medium-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (50W 250° Medium Stress)]]
*[[Media:PECVD2-SiNx -h.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (5W 250° High Stress)]]
*[[Media:28-Very-low-pin-hole-density SiNx film at 300 C.pdf|Very-Low-Pin-Hole-Density SiNx Recipe(25W 300°)]]
|-
|}


==Standard Cleaning Procedure (PECVD #2)==
=== SiN (2% SiH<sub>4</sub> - No-Ar) ===
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#D0E7FF"
! width="350" align="center" |50° (pinholes)
! width="350" align="center" |100° (pinholes)
! width="350" align="center" |250°
|- align="left"
|
*[[Media:PECVD2-SiN-Recipe-NoAr-5W-50C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 50° High Stress)]]
*[[Media:41-High-stress SiNx at 50 C using Unaxis ICP deposition tool.pdf|Film Properties of High-stress SiN<sub>x</sub> (No Ar, 5W, 50°)]]
*[[Media:PECVD2-SiN-Recipe-NoAr-50W-50C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 50° Medium Stress)]]
*[[Media:36-Medium-stress SiNx using Unaxis ICP deposition tool-a.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 50°)]]
*[[Media:PECVD2-SiN-Recipe-NoAr-120W-50C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 50° Low Stress)]]
*[[Media:40-Low-stress SiNx at 50 C using Unaxis ICP deposition tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 50°)]]
|
*[[Media:PECVD2-SiN-Recipe-NoAr-5W-100C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 100° High Stress)]]
*[[Media:38-High-stress SiNx at 100 C using Unaxis ICP deposition tool.pdf|Film Properties of high-stress SiN<sub>x</sub> (No Ar, 5W, 100°)]]
*[[Media:PECVD2-SiN-Recipe-NoAr-50W-100C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 100° Medium Stress)]]
*[[Media:39-Medium-stress SiNx at 100C using Unaxis ICP deposition tool.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 100°)]]
*[[Media:PECVD2-SiN-Recipe-NoAr-120W-100C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 100° Low Stress)]]
*[[Media:37-Low-stress SiNx at 100 C using Unaxis ICP deposition tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 100°)]]
|
*[[Media:PECVD2-SiN-Recipe-NoAr-5W-250C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 250° High Stress)]]
*[[Media:34-High-stress SiNx at 250 C using Unaxis ICP deposition tool.pdf|Film Properties of High-stress SiN<sub>x</sub> (No Ar, 5W, 250°)]]
*[[Media:PECVD2-SiN-Recipe-NoAr-50W-250C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 250° Medium Stress)]]
*[[Media:36-Medium-stress SiNx using Unaxis ICP deposition tool-a.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 250°)]]
*[[Media:PECVD2-SiN-Recipe-NoAr-120W-250C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 250° Low Stress)]]
*[[Media:35-Low-stress SiNx at 250 C using Unaxis ICP deposition tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 250°)]]
|-
|}


#If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
=== SiN (2% SiH<sub>4</sub> - No-Ar - Extra N<sub>2</sub>) ===
#Load the recipe for cleaning "STD CF<sub>4</sub>/O<sub>2</sub> Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#D0E7FF"
! width="350" align="center" |50° (pinholes)
! width="350" align="center" |100° (pinholes)
! width="350" align="center" |250°
|- align="left"
|
*[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-50C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 50° Low Stress)]]
|
*[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-100C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 100° Low Stress)]]
|
*[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-250C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 250° Low Stress)]]
|-
|}


===[https://wiki.nanofab.ucsb.edu/wiki/File:STD_CF4-O2_Clean_PECVD2.jpg Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"]===
=== SiN (100% SiH<sub>4</sub> ) ===
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#D0E7FF"
! width="350" align="center" |50° (pinholes)
! width="350" align="center" |100° (pinholes)
! width="350" align="center" |250°
|- align="left"
|
*[[Media:PECVD2-SiN-Recipe-Low stress SiNx-100%SiH4-120W-50C.pdf|SiN Deposition Recipe (120W 50° Low Stress)]]
|
*[[Media:PECVD2-SiN-Recipe-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Deposition Recipe (120W 100° Low Stress)]]
*[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 120W-100(250)C]]
|
*[[Media:PECVD2-SiN-Recipe-Low stress SiNx-100% SiH4-120W-250C.pdf|SiN Deposition Recipe (120W 250° Low Stress)]]
*[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 120W, 100(250)C]]
|- align="left"
|
*[[Media:PECVD2-SiN-Recipe-Medium stress SiNx-100%SiH4-120W-50C.pdf|SiN Deposition Recipe (50W 50° Medium Stress)]]
|
*[[Media:PECVD2-SiN-Recipe-Medium stres SiNx-100% SiH4-120W-100C.pdf|SiN Deposition Recipe (50W 100° Medium Stress)]]
*[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 50W, 100(250)C]]
*[[Media:27-SiNx_Film_(Bias%3D50W)_Sidewall_Coverage.pdf|SiN SEM sidewall coverage]]
|
*[[Media:PECVD2-SiN-Recipe-Medium stress SiNx-100% SiH4-120W-250C.pdf|SiN Deposition Recipe (50W 250° Medium Stress)]]
*[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN ComparisonTable 50W, 100(250)C]]
|-
|}


==SiO<sub>2</sub> deposition (Unaxis VLR) ==
=== SiO<sub>2</sub> (2% SiH<sub>4</sub>) ===
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#D0E7FF"
! width="350" align="center" |50°
! width="350" align="center" |100°
! width="350" align="center" |250°
|- align="left"
|
*[[Media:PECVD2-SiO2Recipe-5W-50C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 50°)]]
|
*[[Media:PECVD2-SiO2Recipe-5W-100C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 100°)]]
*[[Media:SiO2 film Unaxis ICP vs PECVD I.pdf|SiO<sub>2</sub> film Unaxis ICP vs PECVD I]]
*[[Media:SEM pictures SiO2 100C.pdf|SiO<sub>2</sub> SEM pictures 100C]]
|
*[[Media:PECVD2-SiO2Recipe-5W-250C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 250°)]]
*[[Media:SiO2 film Unaxis ICP vs PECVD I.pdf|SiO<sub>2</sub> film Unaxis ICP vs PECVD I]]
|-
|}


'''Clean Times (PECVD#2''')
=== SiO<sub>2</sub> (2% SiH<sub>4</sub> - No Ar) ===
{| class="wikitable"
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
!Film Deposited
|- bgcolor="#D0E7FF"
!Cleaning Time (Dry)
! width="350" align="center" |50°
! width="350" align="center" |100°
! width="350" align="center" |250°
|- align="left"
|
*[[Media:PECVD2-SiO2-Recipe-NoAr-50C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (50°)]]
*[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]]
|
*[[Media:PECVD2-SiO2-Recipe-NoAr-100C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (100°)]]
*[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]]
|
*[[Media:PECVD2-SiO2-Recipe-NoAr-250C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (250°)]]
*[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]]
|-
|-
|SiO<sub>2</sub>
|}
|1min. clean for every 1min. deposition

=== SiO<sub>2</sub> (100% SiH<sub>4</sub> HDR) ===
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#D0E7FF"
! width="350" align="center" |50°
! width="350" align="center" |100°
! width="350" align="center" |250°
|- align="left"
|
*[[Media:SiO2 100% SiH4 HDR 50C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (50°)]]
|
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-HDR-100C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (100°)]]
*[[Media:PECVD2-SiO2-HDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - HDR (100°)]]
|
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-HDR-250C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (250°)]]
*[[Media:PECVD2-SiO2-HDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - HDR (250°)]]
|-
|-
|Si<sub>3</sub>N<sub>4</sub>
|}
|1min. clean for every 7min. of deposition
|-
|a-Si
|2 min clean for every 1min of deposition
|-
|a-Si (max 60min dep before breaking it up and cleaning the chamber)
|Wet Clean the Upper Lid/Chamber
DI water then Isopropyl Alcohol on chamber wall & portholes
|-
|Other films:(max 60min long dep. in one single run)
|If > 29min total dep time
(Season + Dep)


Wet Clean the Upper Lid/Chamber
=== SiO<sub>2</sub> (100% SiH<sub>4</sub> LDR) ===
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#D0E7FF"
! width="350" align="center" |50°
! width="350" align="center" |100°
! width="350" align="center" |250°
|- align="left"
|
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-50C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (50°)]]
|
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-100C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (100°)]]
*[[Media:PECVD2-SiO2-LDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - LDR (100°)]]
*[[Media:PECVD2-SiO2-SEM-LDR SiO2-100% SiH4-100C-15W.pdf|SiO<sub>2</sub> SEM sidewall coverage]]
|
*[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-250C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (250°)]]
*[[Media:PECVD2-SiO2-LDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - LDR (250°)]]
|-
|}


DI water then Isopropyl Alcohol on chamber wall & portholes
=== Amorphous Si (100%SiH<sub>4</sub> Ar He) ===
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#D0E7FF"
! width="350" align="center" |90°
! width="350" align="center" |250°
|- align="left"
|
*[[Media:02-ICP-PECVD-a-Si Film-90C.pdf|a-Si Deposition Recipe - 90°]]
|
*[[Media:01-ICP-PECVD-a-Si-Deposition Recipe-250C.pdf|a-Si Deposition Recipe - 250°]]
*[[Media:Amorphous Silicon Film Deposition using 12.5W bias on SiO2-Si.pdf|Thick, Defects-free a-Si Film on SiO<sub>2</sub>/Si with a Lower Bias Power]]
|-
|}
|}

=[[ICP-PECVD (Unaxis VLR)]]=
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the [[ICP-PECVD (Unaxis VLR)#Documentation|new procedures]] to ensure low particle counts in the chamber.

The system currently has '''Deuterated Silane (SiD<sub>4</sub>)''' installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.

==Process Control Data (Unaxis ICP-PECVD)==
''Regularly-run depositions and measurements of film properties over time - executed by [https://nanofab.ucsb.edu/workforce NanoFab Interns].''
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Process Control Plots] - ''Plots of all Process Control data''
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub>]

==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==

*[https://docs.google.com/spreadsheets/d/1mobnAIH70a9eFbCkMnza2WfpI2uRUWtLlz0cLK1Ljuo/edit?gid=1554182668#gid=1554182668 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C-new May 2024''

*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.

=== Old Data ===

* [https://docs.google.com/spreadsheets/d/17ft9jrHcCFCp2830RsLwQq5lHuupWATXT91SreG8WYY/edit#gid=143856038 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C - replaced on May 2024''"
* [https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=1199123007 Old Recipe] - 2019

*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_LDR_250C_Deposition_.28Unaxis_VLR.29 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021

==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==

*[https://docs.google.com/spreadsheets/d/1x0mB4ySSUfEAfRehAx7k_k3BJuTMczaRxQgxsTAFfo4/edit?gid=744785272#gid=744785272 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-new May 2024''"
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.

=== Old Data ===
*[https://docs.google.com/spreadsheets/d/13KUlUujEWSLOH54Ibd52YNJPZcAc7ELShI2RAqM6H-Y/edit#gid=117484667 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-replace on May 2024''"
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=1199123007 Old Recipe] - 2019
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_HDR_250C_Deposition_.28Unaxis_VLR.29 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>]

==Gap-Fill SiO<sub>2</sub> [ICP-PECVD]==
''Recipe designed by [https://scholar.google.com/citations?user=kur3-cEAAAAJ&hl=en&oi=ao Warren Jin], please consider our [https://wiki.nanotech.ucsb.edu/wiki/Frequently_Asked_Questions#Publications_acknowledging_the_Nanofab publication policy] if you publish using this recipe.''
'''NOTE:''' Please contact tool [[Tony Bosch|supervisor]] before running this recipe - this recipe must often be scheduled to prevent excessive chamber maintenance.
Able to effectively fill ~1:1 and ~1:2 aspect ratio gaps in Silicon and Glass structures (eg. waveguides/optical gratings) with void-free filling.

The recipe uses a high 400W RF Bias to reduce buildup on corners that causes voids during growth.

*Category = <code>SiO2 GapFill - Std.</code>
*FLOW: <code>SiO2 GapFill 250C</code>
**Will run the sequence <code>SiO2 GapFill 250C 450W</code>. Do not change this!
*STEP (edit TIME only): <code>SiO2 GapFill 250C</code>
*Deposition rate = 99.968nm/min [9/20/23]

==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==

*[https://docs.google.com/spreadsheets/d/18nE-iTLLH4QIq3wadHVgjVuZ215o9xUz_aCX2WDdges/edit?gid=638997025#gid=638997025 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C-new May 2024''"

* [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
** Lists film data, such as dep rate, stress, particle count, refractive index etc.

=== Old Data ===
*[https://docs.google.com/spreadsheets/d/1Np5uJ1bw81MxHlDD0qs5Jh_hj7nCSznQTsSEELlT414/edit?usp=sharing Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C- replaced on May 2024''"

*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Old Recipe] - 2019
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_250C_deposition_.28Unaxis_VLR.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021

==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==

*[https://docs.google.com/spreadsheets/d/1xchMuXlPABSKcW-rMau8B-cw_jnJnwI9qpXqDLUQ8sU/edit?gid=1239658204#gid=1239658204 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C-new May 2024''"
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.

=== Old Data ===
* [https://docs.google.com/spreadsheets/d/1JuQlCU-mozIUJx9z9aQdisIJyFhv1r9AWI8EWeOnsPo/edit#gid=82816489 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C - replaced on May 2024''"
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Old Recipe] - 2019

==Standard Seasoning Procedure [ICP-PECVD]==
You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film].
Seasoning recipes:
*[https://docs.google.com/spreadsheets/d/1S01xgtxFEJ4q7GLHfo-96yYKxer8nGlB/edit?gid=1944526099#gid=1944526099 SiO<sub>2</sub> seasoning - Std ]
*[https://docs.google.com/spreadsheets/d/1S3BFJIn9oAq2bxg6PDe9RY_6Fvkc36ki/edit?gid=1218243940#gid=1218243940 SiN seasoning - Std ]

==Standard Cleaning Procedure [ICP-PECVD]==
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details.

*SiNx etches at 20nm/min
*SiO<sub>2</sub> etches at 40nm/min

===Standard Clean Recipe===

*[https://docs.google.com/spreadsheets/d/1S3DzvJJahNTwGXsn0GDyg2FiourGffiy/edit?gid=2021404224#gid=2021404224 Post Deposition Clean 250C ]

==General Recipe Notes (Unaxis VLR ICP-PECVD)==

*RF1 = Bias
*RF2 = ICP Power
*All recipes start with an Argon pre-clean with 0W bias (gentle), to improve adhesion/nucleation.
*Maximum SiO<sub>2</sub> Dep. thickness allowed: 800nm
**Above this thickness, you must run a chamber clean/season before depositing more onto your product wafer.

Latest revision as of 18:07, 10 December 2025

Back to Vacuum Deposition Recipes.

PECVD 1 (PlasmaTherm 790)

PECVD 1 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #1)

Old Data

SiN deposition (PECVD #1)

Old Data

Low Stress Si3N4 (PECVD#1)

plot of SiN stress and Refractive Index vs. N2 flow.
Example of Si3N4 modified stress via. varying N2 flow.  Refractive index is relatively constant (one outlier), and stress varies continuously from tensile to compressive.  (Demis D. John 2011, Blumenthal Group)

SiOxNy deposition (PECVD #1)

Standard Cleaning Procedure (PECVD #1)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.

The clean is done in two steps:

  1. Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
  2. Load the recipe for plasma cleaning "CF4/O2 Clean" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.
Table of Cleaning Times
Film Dep'd Cleaning Time
SiO2 1 min clean for every 1 min dep
Si3N4 1 min clean for every 7 min dep
SiOxNy Same as SiO2
a-Si Same time as Si3N4

Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.

PECVD 2 (Advanced Vacuum)

PECVD 2 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #2)

  • SiO2 deposition rate at 150C is 35nm/min

SiN deposition (PECVD #2)

Low-Stress SiN deposition (PECVD #2)

Low-Stress Silicon Nitride, Si3N4 (< ±100 MPa)

Low-Stress SiN 3xTime (PECVD #2)

This Low-Stress SiN recipe is more stable over time (months), because each step is 3x longer (so each compressive/tensile layer is thicker), making it less susceptible to RF ignition delays as the grounding strap is etched over time. – 2024-09 Demis & Biljana

Amorphous-Si deposition (PECVD #2)

Standard Cleaning Procedure (PECVD #2)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
  2. Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.

Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


Clean Times (PECVD#2)

Film Deposited Cleaning Time (Dry)
SiO2 1min. clean for every 1min. deposition
Si3N4 1min. clean for every 7min. of deposition
a-Si 2 min clean for every 1min of deposition
a-Si (max 60min dep before breaking it up and cleaning the chamber) Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

Other films:(max 60min long dep. in one single run) If > 29min total dep time

(Season + Dep)

Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

ICP-PECVD (Unaxis VLR)

2020-02: New recipes have been characterized for low particulate count and repeatability.  Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.

Process Control Data (Unaxis ICP-PECVD)

Regularly-run depositions and measurements of film properties over time - executed by NanoFab Interns.

Low Deposition Rate SiO2 [ICP-PECVD]

Old Data

High Deposition Rate SiO2 [ICP-PECVD]

Old Data

Gap-Fill SiO2 [ICP-PECVD]

Recipe designed by Warren Jin, please consider our publication policy if you publish using this recipe.

NOTE: Please contact tool supervisor before running this recipe - this recipe must often be scheduled to prevent excessive chamber maintenance.

Able to effectively fill ~1:1 and ~1:2 aspect ratio gaps in Silicon and Glass structures (eg. waveguides/optical gratings) with void-free filling.

The recipe uses a high 400W RF Bias to reduce buildup on corners that causes voids during growth.

  • Category = SiO2 GapFill - Std.
  • FLOW: SiO2 GapFill 250C
    • Will run the sequence SiO2 GapFill 250C 450W. Do not change this!
  • STEP (edit TIME only): SiO2 GapFill 250C
  • Deposition rate = 99.968nm/min [9/20/23]

Si3N4 [ICP-PECVD]

Old Data

Low Stress Si3N4 [ICP-PECVD]

Old Data

Standard Seasoning Procedure [ICP-PECVD]

You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film]. Seasoning recipes:

Standard Cleaning Procedure [ICP-PECVD]

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min

Standard Clean Recipe

General Recipe Notes (Unaxis VLR ICP-PECVD)

  • RF1 = Bias
  • RF2 = ICP Power
  • All recipes start with an Argon pre-clean with 0W bias (gentle), to improve adhesion/nucleation.
  • Maximum SiO2 Dep. thickness allowed: 800nm