===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>===
{{Recipe Table Explanation}}
<small>''See above [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used dry etches''</small>


===Dry Etching Tools/Materials Table===

==== Process Maturity Ranking ====

* <code>'''R6'''</code> - most mature process with regular calibrations recorded on SPC charts.
* …
* <code>'''R1'''</code> - least mature - only run once ever.

''The Key/Legend for this table's <code>A...R6</code> values is at the [[Dry Etching Recipes#Process Ranking Table|bottom of the page]].''
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
|-
! colspan="15" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
| bgcolor="#eaecf0" |<!-- INTENTIONALLY LEFT BLANK -->
! colspan="18" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
! colspan="2" |'''[[RIE Etching Recipes|RIE Etching]]'''
|- bgcolor="#d0e7ff"
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
|<!-- INTENTIONALLY LEFT BLANK -->
! colspan="3" |'''[[RIE Etching Recipes|RIE Etching]]'''
! colspan="4" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="6" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="5" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
|- bgcolor="#d0e7ff"
|-
! width="65" bgcolor="#d0e7ff" align="center" |'''Material'''
! bgcolor="#d0e7ff" align="center" |'''Material'''
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| width="100" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| width="100" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E646V)</span>]]
| width="100" bgcolor="#daf1ff" |[https://wiki.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#PlasmaTherm.2FSLR_Fluorine_Etcher SLR Fluorine ICP (PlasmaTherm)]
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic 1)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic 2)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
|[[Oxford ICP Etcher (PlasmaPro 100 Cobra)|Oxford ICP (PlasmaPro 100)]]
| width="85" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| width="95" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]]
| width="95" bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean (YES EcoClean)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ag
! bgcolor="#d0e7ff" align="center" |Ag
Line 44: Line 51:
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
|
|
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Al
! bgcolor="#d0e7ff" align="center" |Al
|
|
|[[RIE Etching Recipes|R2]]
|
|
|[[RIE Etching Recipes|A]]
|
|
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)|R1}}
|[[ICP Etching Recipes#Al Etch .28Panasonic 2.29|R2]]
|
|
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 2)}}
|
|
|
|
Line 63: Line 67:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Au
! bgcolor="#d0e7ff" align="center" |Au
Line 82: Line 83:
|
|
|
|
|[[Other Dry Etching Recipes|R3]]
|
|- bgcolor="#ffffff"
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Cr
! bgcolor="#d0e7ff" align="center" |Cr
|
|
|[[RIE Etching Recipes|R2]]
|
|A
|
|
|
|
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}}
|[[ICP Etching Recipes#Cr Etching (Panasonic 2)|R3]]
|A
|
|
|
|
Line 102: Line 99:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Cu
! bgcolor="#d0e7ff" align="center" |Cu
Line 119: Line 114:
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ge
|
|
|
|
Line 124: Line 123:
|
|
|A
|A
|-
|R1
! bgcolor="#d0e7ff" align="center" |Ge
|
|
|
|
Line 131: Line 129:
|
|
|
|
|[[Other Dry Etching Recipes|R2]]
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Mo
|
|
|
|
Line 140: Line 142:
|
|
|
|
|A
|
|
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Mo
|
|
|
|
|
|
|
|
|R1
|-
!Nb
|
|
|
|
|
|
|
|
|A
|R1
|
|
|
|
Line 161: Line 164:
|
|
|
|
|- bgcolor="#ffffff"
|A
|-
! bgcolor="#d0e7ff" align="center" |Ni
! bgcolor="#d0e7ff" align="center" |Ni
|
|
Line 177: Line 179:
|
|
|
|
|[[Other Dry Etching Recipes|R3]]
|-
!Os
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
! bgcolor="#d0e7ff" align="center" |Pt
|
|
|A
|R1
|
|
|
|
Line 192: Line 196:
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Pt
|
|
|
|
Line 199: Line 205:
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
! bgcolor="#d0e7ff" align="center" |Ru
|
|
|
|
Line 207: Line 210:
|
|
|
|
|A
|{{Rl|ICP Etching Recipes|Ru (Ruthenium) Etch (Panasonic 2)}}
|
|
|[[Other Dry Etching Recipes|R3]]
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ru
|
|
|
|
|
|
|
|
|A
|[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R3]]
|
|
|
|
|
|
|
|
|A
|
|
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Si
! bgcolor="#d0e7ff" align="center" |Si
|
|
|
|
|[[ICP Etching Recipes#High Rate Bosch Etch (DSEIII)|R6]], [[ICP Etching Recipes#Silicon: Single-Step, Low Etch Rate, Smooth Sidewall Process (DSEIII)|R3]]
|[[ICP Etching Recipes#Si Etch Recipes (Fluorine ICP Etcher)|R6]]
|
|
|{{rl|ICP Etching Recipes|DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)}}
|{{Rl|ICP Etching Recipes|Si Etching}}
|
|
|R1
|
|
|A
|
|
|
|
|
|
|[[Other Dry Etching Recipes|R3]]
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ta
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
|
|
|A
|A
|-
|R1
! bgcolor="#d0e7ff" align="center" |Ta
|
|
|
|
Line 247: Line 259:
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ti
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}}
|R1
|
|
|
|
Line 256: Line 273:
|
|
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |Ti
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |W
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}}
|[[ICP Etching Recipes#W Etching (Fluorine ICP Etcher)|R3]]
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}}
|A
|R1
|
|
|
|
Line 273: Line 291:
|
|
|
|
|R1
|-
!TiW
|
|
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
|
|
|R3
|
|
|R1
|
|
|
|
|
|
|
|[https://wiki.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|
|
|
|
Line 290: Line 308:
|
|
|
|
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
|
|
|
|
Line 295: Line 315:
|
|
|A
|A
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]]
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
|
|
|
|
Line 302: Line 321:
|
|
|
|
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}}
|A
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}}
|R1
|
|
|
|
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |AlGaAs
|
|
|
|
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|
|
|R1
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}}
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |AlGaAs
|
|
|[[RIE Etching Recipes|R3]]
|
|
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}}
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}}
|
|
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]]
|
|
|
|
Line 332: Line 354:
|
|
|
|
|A
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |AlGaN
! bgcolor="#d0e7ff" align="center" |AlGaN
Line 341: Line 364:
|
|
|
|
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R2]]
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |AlN
|
|
|
|
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |AlN
|
|
|
|
Line 361: Line 384:
|
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|
|
|R1
|-
!BCB
|
|
|
|
Line 371: Line 395:
|
|
|A
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |CdZnTe
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
|
|
|
|
Line 383: Line 404:
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |CdZnTe
|[[RIE Etching Recipes|R3]]
|
|
|
|
Line 389: Line 413:
|
|
|
|
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |GaAs
|
|
|
|
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}}
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}}
|A
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}}
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |GaAs
|
|
|[[RIE Etching Recipes|R3]]
|
|
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}}
|[[ICP Etching Recipes#GaAs Etch .28Panasonic 2.29|R6]]
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]]
|
|
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |GaN
|
|
|
|
|{{rl|RIE Etching Recipes|GaN Etching (RIE 5)}}
|
|
|
|
|R1
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |GaN
|
|
|[[RIE Etching Recipes|R3]]
|A
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
|R1
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R6]]
|
|
|
|
Line 427: Line 450:
|
|
|
|
|A
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |GaSb
! bgcolor="#d0e7ff" align="center" |GaSb
|
|
|
|
|
|
Line 437: Line 459:
|
|
|A
|A
|R1
|R1
|
|
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
|
|
|
|
Line 444: Line 467:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub>
Line 462: Line 483:
|
|
|
|
|R1
|-
!Hf
|
|
|
|
|
|
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |InGaAlAs
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
|
|
|R2
|
|
|
|
|
|
|A
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |InGaAlAs
|[[RIE Etching Recipes|R3]]
|
|
|
|
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |InGaAsP
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
|R1
|
|
|
|
|
|
|
|
|R
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |InGaAsP
|[[RIE Etching Recipes|R3]]
|
|
|
|
Line 503: Line 524:
|
|
|
|
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R3]]
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |InP
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
|
|
|
|
|A
|A
|R
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |InP
|[[RIE Etching Recipes|R3]]
|
|
|
|
|
|
|A
|R1
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R6]]
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
! bgcolor="#d0e7ff" align="center" |ITO
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
|
|
|
|
|
|
|
|
|[[Other Dry Etching Recipes|R3]]
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |ITO
|[[RIE Etching Recipes|R3]]
|
|
|
|
Line 535: Line 556:
|
|
|
|
|R1
|
|
|
|
Line 541: Line 563:
|
|
|
|
|A
|R1
|-
|- bgcolor="#eeffff"
!LiNbO3
!Photoresist
& ARC
|
|
|A
|[https://wiki.nanotech.ucsb.edu/wiki/RIE_Etching_Recipes#Photoresist_and_ARC_.28RIE_5.29 R]
|
|
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_.26_ARC_.28Fluorine_ICP_Etcher.29 R]
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R]
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_etching_.28Panasonic_2.29 R]
|
|
|R1
|
|
|A
|A
|A
|
|
|
|
|
|
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |SiC
|
|
|
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
!Photoresist & Organics
|
|
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}}
|[[RIE Etching Recipes#Photoresist and ARC (RIE 5)|R3]]
|A
|
|
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]]
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R3]
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]]
|
|
|R3
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
|
|
|
|
|
|
|R1
|-
!ARC (Anti Reflective Coating)
|
|
|
|
|
|
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]]
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |SiN
|
|
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}}
|
|
|
|
|A
|
|
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |SiC
|
|
|
|
|
|
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
|
|
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}}
|R1
|
|
|
|
|{{rl|ICP Etching Recipes|SiO2 Etching (Fluorine ICP Etcher)}}
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
|
|
|
|
Line 614: Line 627:
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |SiN
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
|[[ICP Etching Recipes#Si3N4 Etching .28Fluorine ICP Etcher.29|R3]]
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
|A
|[[ICP Etching Recipes#SiNx Etching .28Panasonic 2.29|R3]]
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |SiOxNy
|
|
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
|
|
|
|
|
|
|
|
|A
|A
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
|
|
|
|
|[[ICP Etching Recipes#SiO2 Etch (DSEiii)|R3]]
|[[ICP Etching Recipes#SiO2 Etch Recipes (Fluorine ICP Etcher)|R6]]
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
|[[ICP Etching Recipes#SiO2 Etching .28Panasonic 2.29|R6]]
|
|
|
|
Line 637: Line 658:
|
|
|
|
|[[Other Dry Etching Recipes|R3]]
|A
|-
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
! bgcolor="#d0e7ff" align="center" |SiOxNy
|
|
|
|
|
|
|
|
|A
|R1
|
|
|
|
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A]
|
|
|
|
Line 652: Line 675:
|
|
|
|
|R1
|-
!SU8
|
|
|
|
Line 657: Line 683:
|
|
|A
|A
|-
! bgcolor="#d0e7ff" align="center" |TiN
|
|
|
|
Line 668: Line 692:
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
|
|
|
|
|
|
|
|
|A
|R1
|
|
|
|
|
|
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
|
|
|
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |TiN
|
|
|
|
Line 694: Line 722:
|
|
|
|
|A
|
|R1
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |W-TiW
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
|
|
|
|
Line 702: Line 731:
|
|
|
|
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}}
|A
|
|
|
|
Line 712: Line 739:
|
|
|
|
|
|R1
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub>
Line 729: Line 755:
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |ZnS
! bgcolor="#d0e7ff" align="center" |ZnS
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|[[RIE Etching Recipes|R3]]
|
|
|
|
Line 748: Line 771:
|
|
|
|
|
|R1
|- bgcolor="#eeffff"
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |ZnSe
! bgcolor="#d0e7ff" align="center" |ZnSe
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|[[RIE Etching Recipes|R2]]
|
|
|
|
Line 767: Line 787:
|
|
|
|
|
|R1
|- bgcolor="#ffffff"
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub>
|
|
Line 778: Line 795:
|
|
|
|
|R1
|
|
|
|
Line 785: Line 803:
|
|
|
|
|
|R1
|- bgcolor="#eeffff"
|
|
|
|A
|-
! bgcolor="#d0e7ff" align="center" |'''Material'''
! bgcolor="#d0e7ff" align="center" |'''Material'''
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|SLR Fluorine ICP (PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic E626I)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic E640)]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
|[[Oxford ICP Etcher (PlasmaPro 100 Cobra)|Oxford ICP (PlasmaPro 100)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| width="95" bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean (YES EcoClean)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]]
|}
|}


===Process Ranking Table===
Processes in the table above are ranked by their "''Process Maturity Level''" as follows:
{| class="wikitable"
!Process Level
! colspan="11" |Description of Process Level Ranking
|-
|A
| colspan="11" |Process '''A'''llowed and materials available but never done
|-
|R1
| colspan="11" |Process has been ran at least once
|-
|R2
| colspan="11" |Process has been ran and procedure is documented
|-
|R3
| colspan="11" |Process has been ran, procedure is documented, and data is available
|-
|R4
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''no''' in-Situ control available
|-
|R5
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' in-Situ control available
|-
|R6
| colspan="11" |Process has a documented procedure and control charts/limits available.  Controlled process.
|}
[[Category:Processing]]
[[Category:Processing]]

Latest revision as of 22:16, 23 September 2026

Process Control Data

See above linked page for process control data (dep rate/stress etc. over time), for a selection of often-used dry etches

Dry Etching Tools/Materials Table

Process Maturity Ranking

  • R6 - most mature process with regular calibrations recorded on SPC charts.
  • …
  • R1 - least mature - only run once ever.

The Key/Legend for this table's A...R6 values is at the bottom of the page.

Dry Etching Recipes
RIE Etching ICP Etching Oxygen Plasma Systems Other Dry Etchers
Material RIE 2
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E646V)
ICP Etch 2
(Panasonic E626I)
Oxford ICP (PlasmaPro 100) Ashers
(Technics PEII)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)
Ag R1
Al R2 R1 R2 R1
Au R3
Cr R2 R1 R3 R1
Cu R1
Ge A R1 R2 R1
Mo R1
Nb A R1
Ni R3
Os A R1
Pt R3
Ru A R3 R1
Si R6, R3 R6 R1 R3 R1
Ta A R1 R1
Ti R1 R1 R1
W R3 R1 R1 R1
TiW R3 R1
Al2O3 A R3 R1
Al2O3 (Sapphire) R1 R1 R1
AlGaAs R3 R1 R3 R1
AlGaN R2 R1
AlN R1
BCB A
CdZnTe R3 R1
GaAs R3 R1 R6 R3 R1
GaN R3 R1 R1 R6 R1
GaSb A R1 R1 R1
HfO2 R1
Hf R2
InGaAlAs R3 R1 R1
InGaAsP R3 R3 R1
InP R3 A R1 R6 R3
ITO R3 R1 R1
LiNbO3 R1 R1
Photoresist & Organics R3 R3 R3 R3 R3 R3 R3 R1
ARC (Anti Reflective Coating) R3
SiC R1 R1 R1
SiN R3 R1 R3 R3 R1
SiO2 R3 R6 R1 R6 R3 R1
SiOxNy A R1 R1
SU8 A
Ta2O5 A R1 R1
TiN R1
TiO2 R1
ZnO2 R1
ZnS R3 R1
ZnSe R2 R1
ZrO2 R1 R1
Material RIE 2
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
Oxford ICP (PlasmaPro 100) Ashers
(Technics PEII)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)

Process Ranking Table

Processes in the table above are ranked by their "Process Maturity Level" as follows:

Process Level Description of Process Level Ranking
A Process Allowed and materials available but never done
R1 Process has been ran at least once
R2 Process has been ran and procedure is documented
R3 Process has been ran, procedure is documented, and data is available
R4 Process has a documented procedure with regular (≥4x per year) data no in-Situ control available
R5 Process has a documented procedure with regular (≥4x per year) data and in-Situ control available
R6 Process has a documented procedure and control charts/limits available.  Controlled process.