===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>=== |
===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>=== |
||
<small>''See [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used |
<small>''See above [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used dry etches''</small> |
||
===Dry Etching Tools/Materials Table=== |
===Dry Etching Tools/Materials Table=== |
||
==== Process Maturity Ranking ==== |
|||
*<small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small> |
|||
*<small>'''A''': ''Material is available for use, but no recipes are provided.''</small> |
|||
* <code>'''R6'''</code> - most mature process with regular calibrations recorded on SPC charts. |
|||
* … |
|||
* <code>'''R1'''</code> - least mature - only run once ever. |
|||
''The Key/Legend for this table's <code>A...R6</code> values is at the [[Dry Etching Recipes#Process Ranking Table|bottom of the page]].'' |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
||
|- |
|- |
||
! colspan=" |
! colspan="15" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div> |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
| bgcolor="#eaecf0" |<!-- INTENTIONALLY LEFT BLANK --> |
| bgcolor="#eaecf0" |<!-- INTENTIONALLY LEFT BLANK --> |
||
! colspan=" |
! colspan="2" |'''[[RIE Etching Recipes|RIE Etching]]''' |
||
! colspan=" |
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]''' |
||
! colspan=" |
! colspan="4" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]''' |
||
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]''' |
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]''' |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
! bgcolor="#d0e7ff" align="center" |'''Material''' |
! bgcolor="#d0e7ff" align="center" |'''Material''' |
||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> <span style="font-size: 88%;">(MRC)</span>]] |
|||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ |
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E646V)</span>]] |
||
| bgcolor="#daf1ff" |[[ |
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]] |
|||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
||
| bgcolor="#daf1ff" | |
|||
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
||
| Line 50: | Line 51: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Al |
! bgcolor="#d0e7ff" align="center" |Al |
||
| |
| |
||
|[[RIE Etching Recipes|R2]] |
|||
| |
| |
||
|[[RIE Etching Recipes|A]] |
|||
| |
| |
||
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)|R1}} |
|||
|[[ICP Etching Recipes#Al Etch .28Panasonic 2.29|R2]] |
|||
| |
| |
||
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)}} |
|||
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 2)}} |
|||
| |
| |
||
| |
| |
||
| Line 69: | Line 67: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Au |
! bgcolor="#d0e7ff" align="center" |Au |
||
| Line 88: | Line 83: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes|R3]] |
|||
| |
|||
| |
|||
| |
|||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Cr |
! bgcolor="#d0e7ff" align="center" |Cr |
||
| |
| |
||
|[[RIE Etching Recipes|R2]] |
|||
| |
|||
|A |
|||
| |
| |
||
| |
| |
||
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}} |
||
|[[ICP Etching Recipes#Cr Etching (Panasonic 2)|R3]] |
|||
|A |
|||
| |
| |
||
| |
| |
||
| Line 108: | Line 99: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Cu |
! bgcolor="#d0e7ff" align="center" |Cu |
||
| Line 126: | Line 115: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Ge |
! bgcolor="#d0e7ff" align="center" |Ge |
||
| Line 136: | Line 122: | ||
| |
| |
||
| |
| |
||
| |
|||
|A |
|||
|A |
|A |
||
|R1 |
|||
| |
| |
||
| |
| |
||
| Line 144: | Line 129: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes|R2]] |
|||
| |
| |
||
| |
|R1 |
||
|A |
|||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Mo |
! bgcolor="#d0e7ff" align="center" |Mo |
||
| Line 164: | Line 147: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- |
|- |
||
!Nb |
!Nb |
||
| Line 174: | Line 154: | ||
| |
| |
||
| |
| |
||
| |
|||
|A |
|||
|A |
|A |
||
| |
|R1 |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 202: | Line 179: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes|R3]] |
|||
|- |
|||
!Os |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|||
|- |
|||
!Os |
|||
| |
| |
||
|A |
|||
|R1 |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|A |
|||
|A |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Pt |
|||
| |
| |
||
| |
| |
||
| Line 225: | Line 204: | ||
| |
| |
||
| |
| |
||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Pt |
|||
| |
| |
||
| |
| |
||
| Line 234: | Line 211: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes|R3]] |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ru |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|A |
|||
|[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R3]] |
|||
| |
| |
||
| |
| |
||
| Line 243: | Line 225: | ||
| |
| |
||
| |
| |
||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ru |
|||
| |
| |
||
| |
| |
||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Si |
|||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#High Rate Bosch Etch (DSEIII)|R6]], [[ICP Etching Recipes#Silicon: Single-Step, Low Etch Rate, Smooth Sidewall Process (DSEIII)|R3]] |
|||
|[[ICP Etching Recipes#Si Etch Recipes (Fluorine ICP Etcher)|R6]] |
|||
| |
| |
||
|A |
|||
|{{Rl|ICP Etching Recipes|Ru (Ruthenium) Etch (Panasonic 2)}} |
|||
| |
| |
||
|R1 |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes|R3]] |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ta |
|||
| |
| |
||
| |
| |
||
| Line 263: | Line 251: | ||
| |
| |
||
|A |
|A |
||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Si |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|{{rl|ICP Etching Recipes|DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)}} |
|||
|{{Rl|ICP Etching Recipes|Si_Etching_.28Fluorine_ICP_Etcher.29}} |
|||
| |
| |
||
| |
| |
||
|A |
|||
| |
| |
||
| |
| |
||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ti |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|{{rl| |
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}} |
||
|R1 |
|||
| |
| |
||
|A |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ta |
|||
| |
| |
||
| |
| |
||
| Line 289: | Line 274: | ||
| |
| |
||
| |
| |
||
|A |
|||
|A |
|||
| |
| |
||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |W |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#W Etching (Fluorine ICP Etcher)|R3]] |
|||
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}} |
|||
|R1 |
|||
| |
| |
||
| |
| |
||
| Line 300: | Line 289: | ||
| |
| |
||
| |
| |
||
|A |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ti |
|||
| |
| |
||
| |
| |
||
|R1 |
|||
|- |
|||
!TiW |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|R3 |
|||
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}} |
|||
|A |
|||
| |
| |
||
|R1 |
|||
| |
| |
||
| |
| |
||
| Line 319: | Line 308: | ||
| |
| |
||
| |
| |
||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 328: | Line 315: | ||
| |
| |
||
|A |
|A |
||
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]] |
|||
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R] |
|||
| |
| |
||
| |
| |
||
| Line 336: | Line 323: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub> |
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub> |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 347: | Line 331: | ||
| |
| |
||
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}} |
||
| |
|R1 |
||
| |
| |
||
| |
| |
||
| Line 355: | Line 339: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |AlGaAs |
! bgcolor="#d0e7ff" align="center" |AlGaAs |
||
| |
| |
||
|[[RIE Etching Recipes|R3]] |
|||
| |
| |
||
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}} |
|||
| |
| |
||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}} |
|||
| |
| |
||
| |
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]] |
||
| |
| |
||
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R]] |
|||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
| Line 374: | Line 355: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |AlGaN |
! bgcolor="#d0e7ff" align="center" |AlGaN |
||
| Line 385: | Line 364: | ||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R2]] |
|||
| |
| |
||
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R]] |
|||
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
| Line 393: | Line 371: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |AlN |
! bgcolor="#d0e7ff" align="center" |AlN |
||
| Line 406: | Line 382: | ||
| |
| |
||
| |
| |
||
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
| Line 412: | Line 387: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- |
|- |
||
!BCB |
!BCB |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 423: | Line 395: | ||
| |
| |
||
|A |
|A |
||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
| Line 436: | Line 406: | ||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |CdZnTe |
! bgcolor="#d0e7ff" align="center" |CdZnTe |
||
| |
|[[RIE Etching Recipes|R3]] |
||
| |
| |
||
| |
| |
||
| Line 449: | Line 419: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |GaAs |
! bgcolor="#d0e7ff" align="center" |GaAs |
||
| |
| |
||
|[[RIE Etching Recipes|R3]] |
|||
| |
| |
||
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}} |
|||
| |
| |
||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}} |
|||
|[[ICP Etching Recipes#GaAs Etch .28Panasonic 2.29|R6]] |
|||
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]] |
|||
| |
| |
||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}} |
|||
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}} |
|||
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R]] |
|||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
| Line 469: | Line 435: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |GaN |
! bgcolor="#d0e7ff" align="center" |GaN |
||
| |
| |
||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
|{{rl|RIE Etching Recipes|GaN Etching (RIE 5)}} |
|||
| |
| |
||
| |
| |
||
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
||
| |
|R1 |
||
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29| |
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R6]] |
||
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
| Line 489: | Line 451: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |GaSb |
! bgcolor="#d0e7ff" align="center" |GaSb |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 499: | Line 459: | ||
| |
| |
||
|A |
|A |
||
| |
|R1 |
||
| |
|R1 |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
| Line 508: | Line 467: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub> |
||
| Line 525: | Line 483: | ||
| |
| |
||
| |
| |
||
|R1 |
|||
|- |
|||
!Hf |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|A |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
|||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|R2 |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|A |
|||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|A |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |InGaAsP |
|||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|||
| |
| |
||
| |
| |
||
|R1 |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]] |
|||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |InGaAsP |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
| |
||
| |
| |
||
| Line 566: | Line 524: | ||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R3]] |
|||
|A |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |InP |
|||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|A |
|||
|A |
|||
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]] |
|||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|||
| |
| |
||
| |
| |
||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |InP |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|A |
|||
|R1 |
|||
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R6]] |
|||
| |
| |
||
| |
| |
||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |ITO |
|||
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}} |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes|R3]] |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |ITO |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
| |
||
| |
| |
||
| Line 598: | Line 556: | ||
| |
| |
||
| |
| |
||
|R1 |
|||
| |
| |
||
| |
| |
||
| Line 604: | Line 563: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- |
|- |
||
!LiNbO3 |
!LiNbO3 |
||
| Line 610: | Line 569: | ||
| |
| |
||
| |
| |
||
|R1 |
|||
| |
| |
||
| |
| |
||
| Line 619: | Line 579: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
!Photoresist |
!Photoresist & Organics |
||
& ARC |
|||
| |
| |
||
|[[RIE Etching Recipes#Photoresist and ARC (RIE 5)|R3]] |
|||
|A |
|||
|[https://wiki.nanotech.ucsb.edu/wiki/RIE_Etching_Recipes#Photoresist_and_ARC_.28RIE_5.29 R] |
|||
| |
| |
||
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
|||
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_.26_ARC_.28Fluorine_ICP_Etcher.29 R] |
|||
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 |
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R3] |
||
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]] |
|||
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_etching_.28Panasonic_2.29 R] |
|||
| |
| |
||
|R3 |
|||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|||
| |
| |
||
|R |
|||
| |
| |
||
|R |
|||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- |
|- |
||
!ARC (Anti Reflective Coating) |
|||
!Ru |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
|||
| |
|||
| |
|||
|A |
|||
|[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R]] |
|||
| |
| |
||
| |
| |
||
| Line 665: | Line 614: | ||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |SiC |
! bgcolor="#d0e7ff" align="center" |SiC |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 671: | Line 619: | ||
| |
| |
||
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}} |
||
| |
|R1 |
||
| |
| |
||
| |
| |
||
| Line 679: | Line 627: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |SiN |
! bgcolor="#d0e7ff" align="center" |SiN |
||
| |
| |
||
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}} |
|||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#Si3N4 Etching .28Fluorine ICP Etcher.29|R3]] |
|||
|A |
|||
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
||
| |
|[[ICP Etching Recipes#SiNx Etching .28Panasonic 2.29|R3]] |
||
| |
| |
||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|||
| |
| |
||
|A |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
||
| |
| |
||
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}} |
|||
| |
| |
||
|[[ICP Etching Recipes#SiO2 Etch (DSEiii)|R3]] |
|||
| |
|||
| |
|[[ICP Etching Recipes#SiO2 Etch Recipes (Fluorine ICP Etcher)|R6]] |
||
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
||
| |
|[[ICP Etching Recipes#SiO2 Etching .28Panasonic 2.29|R6]] |
||
| |
| |
||
| |
| |
||
| Line 716: | Line 658: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes|R3]] |
|||
| |
|||
| |
|R1 |
||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}} |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |SiOxNy |
! bgcolor="#d0e7ff" align="center" |SiOxNy |
||
| Line 726: | Line 666: | ||
| |
| |
||
| |
| |
||
| |
|||
|A |
|||
|A |
|A |
||
|R1 |
|||
| |
| |
||
| |
| |
||
| Line 736: | Line 675: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- |
|- |
||
!SU8 |
!SU8 |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 747: | Line 683: | ||
| |
| |
||
|A |
|A |
||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
| Line 760: | Line 694: | ||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 766: | Line 699: | ||
| |
| |
||
|A |
|A |
||
|R1 |
|||
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A] |
|||
| |
| |
||
| |
| |
||
| Line 774: | Line 707: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |TiN |
! bgcolor="#d0e7ff" align="center" |TiN |
||
| Line 792: | Line 723: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
||
| Line 811: | Line 739: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |W-TiW |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}} |
|||
|A |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub> |
||
| Line 849: | Line 755: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |ZnS |
! bgcolor="#d0e7ff" align="center" |ZnS |
||
| |
|[[RIE Etching Recipes|R3]] |
||
| |
| |
||
| |
| |
||
| Line 868: | Line 771: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |ZnSe |
! bgcolor="#d0e7ff" align="center" |ZnSe |
||
| |
|[[RIE Etching Recipes|R2]] |
||
| |
| |
||
| |
| |
||
| Line 887: | Line 787: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
||
| Line 898: | Line 795: | ||
| |
| |
||
| |
| |
||
|R1 |
|||
| |
| |
||
| |
| |
||
| Line 905: | Line 803: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
|||
| |
|||
| |
|||
|A |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |'''Material''' |
! bgcolor="#d0e7ff" align="center" |'''Material''' |
||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> <span style="font-size: 88%;">(MRC)</span>]] |
|||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ |
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
||
| bgcolor="#daf1ff" |[[ |
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]] |
|||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
||
| |
|||
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
||
| Line 931: | Line 822: | ||
|} |
|} |
||
===Process Ranking Table=== |
|||
Processes in the table above are ranked by their "''Process Maturity Level''" as follows: |
|||
{| class="wikitable" |
|||
!Process Level |
|||
! colspan="11" |Description of Process Level Ranking |
|||
|- |
|||
|A |
|||
| colspan="11" |Process '''A'''llowed and materials available but never done |
|||
|- |
|||
|R1 |
|||
| colspan="11" |Process has been ran at least once |
|||
|- |
|||
|R2 |
|||
| colspan="11" |Process has been ran and procedure is documented |
|||
|- |
|||
|R3 |
|||
| colspan="11" |Process has been ran, procedure is documented, and data is available |
|||
|- |
|||
|R4 |
|||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''no''' in-Situ control available |
|||
|- |
|||
|R5 |
|||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' in-Situ control available |
|||
|- |
|||
|R6 |
|||
| colspan="11" |Process has a documented procedure and control charts/limits available. Controlled process. |
|||
|} |
|||
[[Category:Processing]] |
[[Category:Processing]] |
||
Latest revision as of 22:16, 23 September 2026
Process Control Data
See above linked page for process control data (dep rate/stress etc. over time), for a selection of often-used dry etches
Dry Etching Tools/Materials Table
Process Maturity Ranking
R6- most mature process with regular calibrations recorded on SPC charts.- …
R1- least mature - only run once ever.
The Key/Legend for this table's A...R6 values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
| Process Level | Description of Process Level Ranking | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| A | Process Allowed and materials available but never done | ||||||||||
| R1 | Process has been ran at least once | ||||||||||
| R2 | Process has been ran and procedure is documented | ||||||||||
| R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
| R4 | Process has a documented procedure with regular (≥4x per year) data no in-Situ control available | ||||||||||
| R5 | Process has a documented procedure with regular (≥4x per year) data and in-Situ control available | ||||||||||