PECVD Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Biljana (talk | contribs)
Biljana (talk | contribs)
→Si3N4 [ICP-PECVD]: SiN parameters
 
(45 intermediate revisions by 2 users not shown)
Line 10: Line 10:


*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.

=== Old Data ===
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.231.29 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.231.29 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier


Line 16: Line 19:
*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=98787450 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=98787450 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.

=== Old Data ===
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.231.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.231.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier


Line 28: Line 34:


*[https://wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]
*[https://wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] - ''Rate, Index etc.''
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] - ''Lists film data, such as dep rate, stress, particle count, refractive index etc.''
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]


==Standard Cleaning Procedure (PECVD #1)==
==Standard Cleaning Procedure (PECVD #1)==
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.


The clean is done in two steps:
⚫
#Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )

⚫
#Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
⚫
#'''Wet cleaning''' (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
#
⚫
#Load the recipe for plasma cleaning "'''''CF4/O2 Clean'''''" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.


{| class="wikitable"
{| class="wikitable"
Line 44: Line 51:
|-
|-
|SiO<sub>2</sub>
|SiO<sub>2</sub>
|1 min clean for every 1 min dep
|TBD
|-
|-
|Si<sub>3</sub>N<sub>4</sub>
|Si<sub>3</sub>N<sub>4</sub>
|1 min clean for every 7 min dep
|TBD
|-
|-
|SiOxNy
|SiOxNy
|Same as XYZ
|Same as SiO<sub>2</sub>
|-
|a-Si
⚫
|Same time as Si<sub>3</sub>N<sub>4</sub>
|}
|}

#


===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]===
===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]===
Line 65: Line 73:


*[https://docs.google.com/spreadsheets/d/1cYK-k669vf8YO2q2YCGa3gTdaDI3I3M-a9KR5RDlZWY/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD SiO2 v2''"
*[https://docs.google.com/spreadsheets/d/1cYK-k669vf8YO2q2YCGa3gTdaDI3I3M-a9KR5RDlZWY/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD SiO2 v2''"
*[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''STD SiO2''"
**[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''STD SiO2''"
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=1313651154 SiO<sub>2</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=1313651154 SiO<sub>2</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.232.29 SiO<sub>2</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.232.29 SiO<sub>2</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021

*SiO<sub>2</sub> deposition rate at 150C is 35nm/min


==SiN deposition (PECVD #2)==
==SiN deposition (PECVD #2)==


*[https://docs.google.com/spreadsheets/d/1JBXEfRGemFJK81RkHfxS0cTucb3viUL7hMGzmKRD5uU/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD Si3N4 v3''"
*[https://docs.google.com/spreadsheets/d/1JBXEfRGemFJK81RkHfxS0cTucb3viUL7hMGzmKRD5uU/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD Si3N4 v3''"
*[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''Nitride2''"
**[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''Nitride2''"
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=773875841 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=773875841 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.232.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.232.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021


Line 81: Line 93:
*[https://docs.google.com/spreadsheets/d/19VQ6ytYbZ5SsAiXzgWqwlyJUqgjWb8x_eyv7L8DvtwM/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD LS-Si3N4 v4''"
*[https://docs.google.com/spreadsheets/d/19VQ6ytYbZ5SsAiXzgWqwlyJUqgjWb8x_eyv7L8DvtwM/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD LS-Si3N4 v4''"


*[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "'' Old LSNitride2 recipe ''"
**[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "'' Old LSNitride2 recipe ''"


*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=203400760 Plots of Low-Stress Si<sub>3</sub>N<sub>4</sub> Process Control Data]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=203400760 Plots of Low-Stress Si<sub>3</sub>N<sub>4</sub> Process Control Data]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[[Old Deposition Data - 2021-12-15#Low-Stress SiN deposition .28PECVD .232.29|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data - Before Oct. 2021</nowiki>]]
*[[Old Deposition Data - 2021-12-15#Low-Stress SiN deposition .28PECVD .232.29|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data - Before Oct. 2021</nowiki>]]
*:''Old Versions of the recipe:''
*:''Old Versions of the recipe:''
Line 94: Line 107:


*Recipe: "''[https://docs.google.com/spreadsheets/d/1OQp_sux5YEgpcyH3sf0JCwTOhvoi_LSYKOUMRR4Umh4?usp=drive_fs STD LS-Si3N4 3xTime v1]"''
*Recipe: "''[https://docs.google.com/spreadsheets/d/1OQp_sux5YEgpcyH3sf0JCwTOhvoi_LSYKOUMRR4Umh4?usp=drive_fs STD LS-Si3N4 3xTime v1]"''
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?usp=sharing Process Control Data]: Calibration Data
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?usp=sharing Process Control Data]: Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?gid=974005628#gid=974005628 Process Control Charts/Plots]: Calibration control limits versus date
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?gid=974005628#gid=974005628 Process Control Charts/Plots]: Calibration control limits versus date


==Amorphous-Si deposition (PECVD #2)==
==Amorphous-Si deposition (PECVD #2)==


*[[PECVD-2 - a-Si Recipe and Dep process (2025)|a-Si Recipe and Dep process]] 2025-11
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe]
**''Developed by Ryan Hersey & Skyler Palatnik, Group of Prof. Max Millar-Blanchaer''
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Film Characterization and Stress]
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe] (2013-09, Ning Cao)
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Film - Characterization and Stress] - DOE/recipe variations


==Standard Cleaning Procedure (PECVD #2)==
==Standard Cleaning Procedure (PECVD #2)==
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:


#(If >29min dep time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again.
#If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
#Load the recipe for cleaning "STD CF<sub>4</sub>/O<sub>2</sub> Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.
#Load the recipe for cleaning "STD CF<sub>4</sub>/O<sub>2</sub> Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.


===[https://wiki.nanotech.ucsb.edu/w/images/3/34/PECVD2_photo_for_cleaning.png Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"]===
===[https://wiki.nanofab.ucsb.edu/wiki/File:STD_CF4-O2_Clean_PECVD2.jpg Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"]===
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


Line 118: Line 133:
|-
|-
|SiO<sub>2</sub>
|SiO<sub>2</sub>
|1 min. clean for every 1 min. deposition
|1min. clean for every 1min. deposition
|-
|-
|Si<sub>3</sub>N<sub>4</sub>
|Si<sub>3</sub>N<sub>4</sub>
|1 min. clean for every 7 min of deposition
|1min. clean for every 7min. of deposition
|-
|-
|a-Si
|2 min clean for every 1min of deposition
|-
|a-Si (max 60min dep before breaking it up and cleaning the chamber)
⚫
|Wet Clean the Upper Lid/Chamber
DI water then Isopropyl Alcohol on chamber wall & portholes
|-
|Other films:(max 60min long dep. in one single run)
|If > 29min total dep time
|If > 29min total dep time
(Season + Dep)
(Season + Dep)

⚫
|Wet Clean the Upper Lid/Chamber
Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes
DI water then Isopropyl Alcohol on chamber wall & portholes
|}
|}
Line 135: Line 160:


==Process Control Data (Unaxis ICP-PECVD)==
==Process Control Data (Unaxis ICP-PECVD)==
''Regularly-run depositions and measurements of film properties over time - executed by [https://nanofab.ucsb.edu/workforce NanoFab Interns].''

*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Process Control Plots] - ''Plots of all Process Control data''
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Process Control Plots] - ''Plots of all Process Control data''
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub>]
Line 144: Line 169:
==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==
==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==


*[https://docs.google.com/spreadsheets/d/17ft9jrHcCFCp2830RsLwQq5lHuupWATXT91SreG8WYY/edit#gid=143856038 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C-until May 2024''"
*[https://docs.google.com/spreadsheets/d/1mobnAIH70a9eFbCkMnza2WfpI2uRUWtLlz0cLK1Ljuo/edit?gid=1554182668#gid=1554182668 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C-new May 2024''
⚫
*[https://docs.google.com/spreadsheets/d/1mobnAIH70a9eFbCkMnza2WfpI2uRUWtLlz0cLK1Ljuo/edit?gid=1554182668#gid=1554182668 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C-after May 2024''"

⚫
**[https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=1199123007 Old Recipe] -


*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_LDR_250C_Deposition_.28Unaxis_VLR.29 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021


=== Old Data ===
⚫
==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==


*[https://docs.google.com/spreadsheets/d/13KUlUujEWSLOH54Ibd52YNJPZcAc7ELShI2RAqM6H-Y/edit#gid=117484667 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-until May 2024''"
* [https://docs.google.com/spreadsheets/d/17ft9jrHcCFCp2830RsLwQq5lHuupWATXT91SreG8WYY/edit#gid=143856038 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C - replaced on May 2024''"
*[https://docs.google.com/spreadsheets/d/1x0mB4ySSUfEAfRehAx7k_k3BJuTMczaRxQgxsTAFfo4/edit?gid=744785272#gid=744785272 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-after May 2024''"
* [https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=1199123007 Old Recipe] - 2019


⚫
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_LDR_250C_Deposition_.28Unaxis_VLR.29 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021
⚫
**[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=1199123007 Old Recipe]


⚫
==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==

⚫
*[https://docs.google.com/spreadsheets/d/1x0mB4ySSUfEAfRehAx7k_k3BJuTMczaRxQgxsTAFfo4/edit?gid=744785272#gid=744785272 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-new May 2024''"
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.

=== Old Data ===
⚫
*[https://docs.google.com/spreadsheets/d/13KUlUujEWSLOH54Ibd52YNJPZcAc7ELShI2RAqM6H-Y/edit#gid=117484667 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-replace on May 2024''"
⚫
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=1199123007 Old Recipe] - 2019
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_HDR_250C_Deposition_.28Unaxis_VLR.29 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>]
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_HDR_250C_Deposition_.28Unaxis_VLR.29 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>]


Line 173: Line 203:
**Will run the sequence <code>SiO2 GapFill 250C 450W</code>. Do not change this!
**Will run the sequence <code>SiO2 GapFill 250C 450W</code>. Do not change this!
*STEP (edit TIME only): <code>SiO2 GapFill 250C</code>
*STEP (edit TIME only): <code>SiO2 GapFill 250C</code>
*Deposition rate = 99.968nm/min [9/20/23]


==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==
==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==


*[https://docs.google.com/spreadsheets/d/1MffAE2S-Sga0o4botssPMi_P8C2ghxw4XiHwTnOn95Q/edit#gid=1111781219 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C- until May 2024''"
* [https://docs.google.com/spreadsheets/d/1xvXqgFaKT6vH4ZSAfOaqAYnx_qyEqzNZFqTc-OGENzw/edit?gid=1168016715#gid=1168016715 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD]- Standard Recipe</nowiki>] - ''"SiN 250C-v2- New recipe since April 2026"''
**recipe "SiN 250C-v2", sequence "SiN 250C-v2", category "SiN Std."
**this film has a low particle count (good for waveguides)
**requires 30sec O2 plasma using PE-II beforehand
**dep.rate=90.86nm/min, refractive index at 632.8nm=2.04372, refractive index at 1550nm=2.00804, stress=-183MPa
**Cauchy A=2.004+/-0.0013, B=0.00745+/-0.00072928, C=0.00999+/-0.00011018


*[https://docs.google.com/spreadsheets/d/18nE-iTLLH4QIq3wadHVgjVuZ215o9xUz_aCX2WDdges/edit?gid=638997025#gid=638997025 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C-after May 2024''"
* *[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit?gid=1670372499#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
** Lists film data, such as dep rate, stress, particle count, refractive index etc.


=== Old Data ===
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Old Recipe]
*[https://docs.google.com/spreadsheets/d/1Np5uJ1bw81MxHlDD0qs5Jh_hj7nCSznQTsSEELlT414/edit?usp=sharing Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C- replaced on May 2024''"


*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Old Recipe] - 2019
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_250C_deposition_.28Unaxis_VLR.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_250C_deposition_.28Unaxis_VLR.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021


** Lists film data, such as dep rate, stress, particle count, refractive index etc.
⚫
==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==


*[https://docs.google.com/spreadsheets/d/1JuQlCU-mozIUJx9z9aQdisIJyFhv1r9AWI8EWeOnsPo/edit#gid=82816489 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C-until May 2024''"
==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==

⚫
* [https://docs.google.com/spreadsheets/d/1xchMuXlPABSKcW-rMau8B-cw_jnJnwI9qpXqDLUQ8sU/edit?gid=1239658204#gid=1239658204 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C-after May 2024''"

**[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Old Recipe]


*[https://docs.google.com/spreadsheets/d/1xchMuXlPABSKcW-rMau8B-cw_jnJnwI9qpXqDLUQ8sU/edit?gid=1239658204#gid=1239658204 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C-new May 2024''"
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.

=== Old Data ===
* [https://docs.google.com/spreadsheets/d/1JuQlCU-mozIUJx9z9aQdisIJyFhv1r9AWI8EWeOnsPo/edit#gid=82816489 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C - replaced on May 2024''"
⚫
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Old Recipe] - 2019


==Standard Seasoning Procedure [ICP-PECVD]==
==Standard Seasoning Procedure [ICP-PECVD]==
You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film]. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details.
You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film].
Seasoning recipes:
Seasoning recipes:
*[https://docs.google.com/spreadsheets/d/1S01xgtxFEJ4q7GLHfo-96yYKxer8nGlB/edit?gid=1944526099#gid=1944526099 SiO<sub>2</sub> seasoning - Std ]
*[https://docs.google.com/spreadsheets/d/1S01xgtxFEJ4q7GLHfo-96yYKxer8nGlB/edit?gid=1944526099#gid=1944526099 SiO<sub>2</sub> seasoning - Std ]
Line 208: Line 248:


===Standard Clean Recipe===
===Standard Clean Recipe===

''To Be Added''
*[https://docs.google.com/spreadsheets/d/1S3DzvJJahNTwGXsn0GDyg2FiourGffiy/edit?gid=2021404224#gid=2021404224 Post Deposition Clean 250C ]


==General Recipe Notes (Unaxis VLR ICP-PECVD)==
==General Recipe Notes (Unaxis VLR ICP-PECVD)==

Latest revision as of 21:34, 28 September 2026

Back to Vacuum Deposition Recipes.

PECVD 1 (PlasmaTherm 790)

PECVD 1 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #1)

Old Data

SiN deposition (PECVD #1)

Old Data

Low Stress Si3N4 (PECVD#1)

plot of SiN stress and Refractive Index vs. N2 flow.
Example of Si3N4 modified stress via. varying N2 flow.  Refractive index is relatively constant (one outlier), and stress varies continuously from tensile to compressive.  (Demis D. John 2011, Blumenthal Group)

SiOxNy deposition (PECVD #1)

Standard Cleaning Procedure (PECVD #1)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.

The clean is done in two steps:

  1. Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
  2. Load the recipe for plasma cleaning "CF4/O2 Clean" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.
Table of Cleaning Times
Film Dep'd Cleaning Time
SiO2 1 min clean for every 1 min dep
Si3N4 1 min clean for every 7 min dep
SiOxNy Same as SiO2
a-Si Same time as Si3N4

Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.

PECVD 2 (Advanced Vacuum)

PECVD 2 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #2)

  • SiO2 deposition rate at 150C is 35nm/min

SiN deposition (PECVD #2)

Low-Stress SiN deposition (PECVD #2)

Low-Stress Silicon Nitride, Si3N4 (< ±100 MPa)

Low-Stress SiN 3xTime (PECVD #2)

This Low-Stress SiN recipe is more stable over time (months), because each step is 3x longer (so each compressive/tensile layer is thicker), making it less susceptible to RF ignition delays as the grounding strap is etched over time. – 2024-09 Demis & Biljana

Amorphous-Si deposition (PECVD #2)

Standard Cleaning Procedure (PECVD #2)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
  2. Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.

Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


Clean Times (PECVD#2)

Film Deposited Cleaning Time (Dry)
SiO2 1min. clean for every 1min. deposition
Si3N4 1min. clean for every 7min. of deposition
a-Si 2 min clean for every 1min of deposition
a-Si (max 60min dep before breaking it up and cleaning the chamber) Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

Other films:(max 60min long dep. in one single run) If > 29min total dep time

(Season + Dep)

Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

ICP-PECVD (Unaxis VLR)

2020-02: New recipes have been characterized for low particulate count and repeatability.  Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.

Process Control Data (Unaxis ICP-PECVD)

Regularly-run depositions and measurements of film properties over time - executed by NanoFab Interns.

Low Deposition Rate SiO2 [ICP-PECVD]

Old Data

High Deposition Rate SiO2 [ICP-PECVD]

Old Data

Gap-Fill SiO2 [ICP-PECVD]

Recipe designed by Warren Jin, please consider our publication policy if you publish using this recipe.

NOTE: Please contact tool supervisor before running this recipe - this recipe must often be scheduled to prevent excessive chamber maintenance.

Able to effectively fill ~1:1 and ~1:2 aspect ratio gaps in Silicon and Glass structures (eg. waveguides/optical gratings) with void-free filling.

The recipe uses a high 400W RF Bias to reduce buildup on corners that causes voids during growth.

  • Category = SiO2 GapFill - Std.
  • FLOW: SiO2 GapFill 250C
    • Will run the sequence SiO2 GapFill 250C 450W. Do not change this!
  • STEP (edit TIME only): SiO2 GapFill 250C
  • Deposition rate = 99.968nm/min [9/20/23]

Si3N4 [ICP-PECVD]

  • Si3N4 [ICP-PECVD]- Standard Recipe - "SiN 250C-v2- New recipe since April 2026"
    • recipe "SiN 250C-v2", sequence "SiN 250C-v2", category "SiN Std."
    • this film has a low particle count (good for waveguides)
    • requires 30sec O2 plasma using PE-II beforehand
    • dep.rate=90.86nm/min, refractive index at 632.8nm=2.04372, refractive index at 1550nm=2.00804, stress=-183MPa
    • Cauchy A=2.004+/-0.0013, B=0.00745+/-0.00072928, C=0.00999+/-0.00011018

Old Data

    • Lists film data, such as dep rate, stress, particle count, refractive index etc.

Low Stress Si3N4 [ICP-PECVD]

Old Data

Standard Seasoning Procedure [ICP-PECVD]

You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film]. Seasoning recipes:

Standard Cleaning Procedure [ICP-PECVD]

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min

Standard Clean Recipe

General Recipe Notes (Unaxis VLR ICP-PECVD)

  • RF1 = Bias
  • RF2 = ICP Power
  • All recipes start with an Argon pre-clean with 0W bias (gentle), to improve adhesion/nucleation.
  • Maximum SiO2 Dep. thickness allowed: 800nm
    • Above this thickness, you must run a chamber clean/season before depositing more onto your product wafer.