OLD Direct-Write I-Line Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Biljana (talk | contribs)
MLa recipes- Bilja trying to link R to recipes
 
note redirecting to new page
 
(25 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''OLD PAGE''': please use this one instead: [[Direct-Write Lithography Recipes#Maskless Aligner (Heidelberg MLA150)|Direct-Write Lithography Recipes#'''Maskless Aligner (Heidelberg MLA150)''']]
All recipes are being merged into the above page, the below info is old. 2026-10-01 [[Demis D. John|DJ]]

__TOC__

==[[Maskless Aligner (Heidelberg MLA150)]]==
==[[Maskless Aligner (Heidelberg MLA150)]]==
Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]]. ''Description of litho params- different lasers available, greyscale etc.''
Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]]. ''Description of litho params- different lasers available, greyscale etc.''
===Positive Resist (MLA150)===
===Positive Resist (MLA150)===
''General notes: Hotplates used, filters, laser wavelengths, etc.''
''General notes: Hotplates used, filters, laser wavelengths, etc. “Soft Bake” is right after spin, “PEB” is post-exposure bake - right after exposure''
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"
|- bgcolor="#D0E7FF"
|- bgcolor="#D0E7FF"
! width="100" |Resist
! width="100" |Resist
! width="100" |Spin Cond.
! width="100" |Spin Cond.
! width="75" |Bake
! width="75" |Soft Bake
! width="75" |Thickness
! width="75" |Thickness
!Laser (nm)
!Laser (nm)
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
! width="100" |DeFocus
! width="100" |DeFocus
! width="75" |PEB
! width="75" |Post-Exposure Bake
! width="100" |Developer
! width="100" |Developer
! width="125" |Developer Time
! width="125" |Developer Time
Line 52: Line 57:
|
|
|
|
|-
|[[:File:SPR220-Positive-Resist-Datasheet.pdf|SPR 955 1.8]]
|4 krpm/30s
|95°C/60”
|~1.8 µm
|405
|210
| 10
|110°C/60s
|AZ300MIF
|60s
|UCSB design (good for dense lines~1um)
|-
|-
|[[:File:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-3.0]]
|[[:File:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-3.0]]
Line 64: Line 81:
|60s
|60s
|Used MLA design
|Used MLA design
|-
|[[:File:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-7.0]]
|3.5 krpm/30s
|115°C/2m
|~7 µm
|405
|440
|5
|50°C/1m, ramp up, 115°C/90s
|AZ300MIF
|70s
|UCSB design 1um pillars/5um trenches]
|-
|-
|[[:File:SPR955-Positive-Resist-Datasheet.pdf|SPR 955-CM0.9]]
|[[:File:SPR955-Positive-Resist-Datasheet.pdf|SPR 955-CM0.9]]
|3 krpm/30s
|3 krpm/30s
|95°C/90”
|95°C/60”
|~ 0.9 µm
|~ 0.9 µm
|405
|405
|250
|250
| - 7
| - 7
|110°C/90s
|110°C/60s
|AZ300MIF
|AZ300MIF
|60s
|60s
|Used MLA design
|Used MLA design, [for 5um pillars/1um trench:150/5]
|-
|-
|[[:File:3600 D, D2v Spin Speed Curve.pdf|THMR-3600HP]]
|[[:File:3600 D, D2v Spin Speed Curve.pdf|THMR-3600HP]]
Line 89: Line 118:
|line/space:
|line/space:
low dose for clear-field, high does for dark-field
low dose for clear-field, high does for dark-field
|-
|[[:File:3600 D, D2v Spin Speed Curve.pdf|THMR-3600HP]]
|6 krpm/30sec
|100°C/60s
|0.260µm
|405
|190
|<nowiki>-4</nowiki>
|100°C/60s
|AZ300MiF
|20s
|Big pattern (>2um), dense
|}
|}

===Negative Resist (MLA150)===
===Negative Resist (MLA150)===
''General notes: Hotplates used, filters, laser wavelengths, etc.''
''General notes: Hotplates used, filters, laser wavelengths, etc. “Soft Bake” is right after spin, “PEB” is post-exposure bake - right after exposure. “Flood exposure” is only for AZ5214 for image reversal, after PEB.''
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"
|- bgcolor="#D0E7FF"
|- bgcolor="#D0E7FF"
! width="100" |Resist
! width="100" |Resist
! width="100" |Spin Cond.
! width="100" |Spin Cond.
! width="75" |Bake
! width="75" |Soft Bake
! width="75" |Thickness
! width="75" |Thickness
!Laser (nm)
!Laser (nm)
Line 154: Line 196:
! width="75" |Bake
! width="75" |Bake
! width="75" |Thickness
! width="75" |Thickness
! width="75" |Laser
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
! width="100" |Focus Offset
! width="100" |Focus Offset
! width="75" |Rehydrate
! width="75" |PEB
! width="75" |PEB
! width="75" |Flood
! width="75" |Flood
Line 165: Line 209:
|– krpm/30”
|– krpm/30”
|95°C/60”
|95°C/60”
|
|
|
|
|
Line 174: Line 219:
| align="left" |
| align="left" |
*TBD
*TBD
|-
|SPR 220-7
|–3.5krpm/30”
|105°C/120” Cool 1min
|~7um
|375
|624mJ to clear large mm area, 520mJ to clear ~5um lines
|neg 20
|>1hr
|115C/90s
|AZ300MIF
|70s
|align="left"|
*TBD
|Rehydration after exposure is necessary, to prevent bubbles at PEB
|}
|}

Latest revision as of 23:22, 1 October 2026

OLD PAGE: please use this one instead: Direct-Write Lithography Recipes#Maskless Aligner (Heidelberg MLA150) 
All recipes are being merged into the above page, the below info is old. 2026-10-01 DJ

Maskless Aligner (Heidelberg MLA150)

Photolithography Recipes for the Heidelberg MLA150. Description of litho params- different lasers available, greyscale etc.

Positive Resist (MLA150)

General notes: Hotplates used, filters, laser wavelengths, etc. “Soft Bake” is right after spin, “PEB” is post-exposure bake - right after exposure

Resist Spin Cond. Soft Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus Post-Exposure Bake Developer Developer Time Comments
AZ4110 4 krpm/30s 95°C/60s ~ 1.1 µm 405 240 5 none AZ400K:DI 1:4 50s Used MLA design (good for isolated lines 0.8-1um)
AZ4330 4 krpm/30s 95°C/60s ~ 3.3 µm 405 320 6 none AZ400K:DI 1:4 90s Used MLA design
AZ4620
SPR 955 1.8 4 krpm/30s 95°C/60” ~1.8 µm 405 210 10 110°C/60s AZ300MIF 60s UCSB design (good for dense lines~1um)
SPR 220-3.0 2.5 krpm/30s 115°C/90” ~ 2.7 µm 405 325 - 4 115°C/90s AZ300MIF 60s Used MLA design
SPR 220-7.0 3.5 krpm/30s 115°C/2m ~7 µm 405 440 5 50°C/1m, ramp up, 115°C/90s AZ300MIF 70s UCSB design 1um pillars/5um trenches]
SPR 955-CM0.9 3 krpm/30s 95°C/60” ~ 0.9 µm 405 250 - 7 110°C/60s AZ300MIF 60s Used MLA design, [for 5um pillars/1um trench:150/5]
THMR-3600HP 1.5 krpm/45s250 rpm/s 100°C/60s 0.430µm 405 180–220 -4 100°C/60s AZ300MiF 20s line/space:

low dose for clear-field, high does for dark-field

THMR-3600HP 6 krpm/30sec 100°C/60s 0.260µm 405 190 -4 100°C/60s AZ300MiF 20s Big pattern (>2um), dense

Negative Resist (MLA150)

General notes: Hotplates used, filters, laser wavelengths, etc. “Soft Bake” is right after spin, “PEB” is post-exposure bake - right after exposure. “Flood exposure” is only for AZ5214 for image reversal, after PEB.

Resist Spin Cond. Soft Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus PEB Flood Developer Developer Time Comments
AZ5214 6 krpm/30s 95°C/60s ~ 1.0 µm 375 35 - 5 110°C/60s 60" AZ300MIF 60s Used UCSB design. Good for up to ~1.3um open line space.
AZnLOF2020 4 krpm/30s 110°C/60s ~ 2.1µm 375 340 - 3 110°C/60s none AZ300MIF 90s Used UCSB design. Good for 2um open line space.
SU-8 2075 ~70µm 375 Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end.

Greyscale Lithography (MLA150)

Description...

Resist Spin Cond. Bake Thickness Laser Exposure Dose (mJ/cm2) Focus Offset Rehydrate PEB Flood Developer Developer Time Comments
AZ4620 – krpm/30” 95°C/60” 60" AZ300MIF 60"
  • TBD
SPR 220-7 –3.5krpm/30” 105°C/120” Cool 1min ~7um 375 624mJ to clear large mm area, 520mJ to clear ~5um lines neg 20 >1hr 115C/90s AZ300MIF 70s
  • TBD
Rehydration after exposure is necessary, to prevent bubbles at PEB