Sputtering Recipes: Difference between revisions
Jump to navigation
Jump to search
(→TiO{{sub|2}} deposition (IBD): rates & indices) |
|||
Line 33: | Line 33: | ||
==TiO{{sub|2}} deposition (IBD)== |
==TiO{{sub|2}} deposition (IBD)== |
||
* Refractive Index ≈ 2.3-2.4 |
* Refractive Index ≈ 2.3-2.4 |
||
* |
* Rate ≈ 1.8nm/min |
||
*{{fl|IBD-TiO2-Recipe.pdf|Recipe: TiO{{sub|2}}_dep}} |
*{{fl|IBD-TiO2-Recipe.pdf|Recipe: TiO{{sub|2}}_dep}} |
Revision as of 20:12, 13 August 2013
Back to Vacuum Deposition Recipes.
Sputter 1 (Custom)
Sputter 2 (SFI Endeavor)
Sputter 3 (AJA ATC 2000-F)
Sputter 4 (AJA ATC 2200-V)
Sputter 5 (Lesker AXXIS)
Ion Beam Deposition (Veeco NEXUS)
IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc. All users are required to enter their calibration deps (simple test deps only)
SiO2 deposition (IBD)
- Refractive Index: ≈1.485
- Rate: ≈6.1nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -320MPa (compressive)
Si3N4 deposition (IBD)
- Refractive Index ≈ 2.01
- Rate ≈ 4.5nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -1756MPa (compressive)
Ta2O5 deposition (IBD)
- Refractive Index ≈ 2.10
- Rate ≈7.8nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -140MPa (compressive)
TiO2 deposition (IBD)
- Refractive Index ≈ 2.3-2.4
- Rate ≈ 1.8nm/min
- Recipe: TiO2_dep