Sputtering Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Line 6: Line 6:
=[[Sputter 5 (Lesker AXXIS)]]=
=[[Sputter 5 (Lesker AXXIS)]]=
=[[Ion Beam Deposition (Veeco NEXUS)]]=
=[[Ion Beam Deposition (Veeco NEXUS)]]=
[https://docs.google.com/spreadsheet/ccc?key=0AuBs1GfMrpnXcEdXanZQNko3X0lUcHhVUlNyYnVDUkE&usp=sharing IBD Calibrations Spreadsheet] - Records of historical film depositions (rates, indices), Uniformity etc. '''All users are required to enter their calibration deps (simple test deps only)'''
[https://docs.google.com/spreadsheet/ccc?key=0AuBs1GfMrpnXcEdXanZQNko3X0lUcHhVUlNyYnVDUkE&usp=sharing IBD Calibrations Spreadsheet] - Records of historical film depositions (rates, indices), Uniformity etc.

'''All users are required to enter their calibration deps (simple test deps only)'''


==SiO{{sub|2}} deposition (IBD)==
==SiO{{sub|2}} deposition (IBD)==

Revision as of 20:12, 13 August 2013

Back to Vacuum Deposition Recipes.

Sputter 1 (Custom)

Sputter 2 (SFI Endeavor)

Sputter 3 (AJA ATC 2000-F)

Sputter 4 (AJA ATC 2200-V)

Sputter 5 (Lesker AXXIS)

Ion Beam Deposition (Veeco NEXUS)

IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc.

All users are required to enter their calibration deps (simple test deps only)

SiO2 deposition (IBD)

  • Refractive Index: ≈1.485
  • Rate: ≈6.1nm/min (users must calibrate this prior to critical deps)
  • Stress ≈ -320MPa (compressive)

Si3N4 deposition (IBD)

  • Refractive Index ≈ 2.01
  • Rate ≈ 4.5nm/min (users must calibrate this prior to critical deps)
  • Stress ≈ -1756MPa (compressive)

Ta2O5 deposition (IBD)

  • Refractive Index ≈ 2.10
  • Rate ≈7.8nm/min (users must calibrate this prior to critical deps)
  • Stress ≈ -140MPa (compressive)

TiO2 deposition (IBD)