===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>=== |
|||
{{Recipe Table Explanation}} |
|||
<small>''See above [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used dry etches''</small> |
|||
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" |
|||
|- bgcolor="#D0E7FF" |
|||
===Dry Etching Tools/Materials Table=== |
|||
! colspan="16" width="725" height="45" | <div style="font-size: 150%;">Dry Etching Recipes</div> |
|||
|- bgcolor="#D0E7FF" |
|||
==== Process Maturity Ranking ==== |
|||
| <!-- INTENTIONALLY LEFT BLANK --> |
|||
! colspan="4" width="300" bgcolor="#D0E7FF" align="center" height="35" | '''[[RIE Etching Recipes|RIE Etching]]''' |
|||
* <code>'''R6'''</code> - most mature process with regular calibrations recorded on SPC charts. |
|||
! colspan="4" width="300" bgcolor="#D0E7FF" align="center" | '''[[ICP Etching Recipes|ICP Etching]]''' |
|||
* … |
|||
! colspan="4" bgcolor="#D0E7FF" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]''' |
|||
* <code>'''R1'''</code> - least mature - only run once ever. |
|||
! colspan="3" bgcolor="#D0E7FF" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]''' |
|||
|- |
|||
''The Key/Legend for this table's <code>A...R6</code> values is at the [[Dry Etching Recipes#Process Ranking Table|bottom of the page]].'' |
|||
! width="65" bgcolor="#D0E7FF" align="center" | '''Material''' |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
|||
| width="65" bgcolor="#DAF1FF" | [[RIE 1 (Custom)|RIE 1<br>(Retired)]] |
|||
|- |
|||
| width="65" bgcolor="#DAF1FF" | [[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]] |
|||
! colspan="15" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div> |
|||
| width="65" bgcolor="#DAF1FF" | [[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]] |
|||
|- bgcolor="#d0e7ff" |
|||
| width="100" bgcolor="#DAF1FF" | [[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]] |
|||
| bgcolor="#eaecf0" |<!-- INTENTIONALLY LEFT BLANK --> |
|||
| width="100" bgcolor="#DAF1FF" | [[ICP_Etching_Recipes#Si_Deep_RIE_.28PlasmaTherm.2FBosch_Etch.29|Si Deep RIE<br>(PTI/Bosch)]] |
|||
! colspan="2" |'''[[RIE Etching Recipes|RIE Etching]]''' |
|||
| width="120" bgcolor="#DAF1FF" | [[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic 1)]] |
|||
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]''' |
|||
| width="120" bgcolor="#DAF1FF" | [[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic 2)]] |
|||
! colspan="4" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]''' |
|||
| width="85" bgcolor="#DAF1FF" | [[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]] |
|||
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]''' |
|||
| width="85" bgcolor="#DAF1FF" | [[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]] |
|||
|- bgcolor="#d0e7ff" |
|||
| width="95" bgcolor="#DAF1FF" | [[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]] |
|||
! bgcolor="#d0e7ff" align="center" |'''Material''' |
|||
| width="85" bgcolor="#DAF1FF" | [[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
|||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
|||
| width="85" bgcolor="#DAF1FF" | [[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]] |
|||
| |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
|||
| width="85" bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]] |
|||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
|||
| width="85" bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]] |
|||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E646V)</span>]] |
|||
|- bgcolor="#EEFFFF" |
|||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
|||
! bgcolor="#D0E7FF" align="center" | Ag |
|||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
|||
| |
|||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
|||
| |
|||
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
|||
| |
|||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
|||
| |
|||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]] |
|||
| |
|||
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]] |
|||
| |
|||
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]] |
|||
| |
|||
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]] |
|||
| |
|||
|- bgcolor="#eeffff" |
|||
| |
|||
! bgcolor="#d0e7ff" align="center" |Ag |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | Al |
|||
| |
|||
| |
|||
| |
|||
| [[RIE Etching Recipes|A]] |
|||
| |
|||
| {{rl|ICP Etching Recipes|Al Etch(Panasonic 1)}} |
|||
| {{rl|ICP Etching Recipes|Al Etch(Panasonic 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
|||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | Au |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | Cr |
|||
| |
|||
| |
|||
| |
|||
| A |
|||
| |
|||
| {{rl|ICP Etching Recipes|Cr Etch(Panasonic 1)}} |
|||
| A |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | Cu |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | Ge |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | Mo |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | Ni |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
|R1 |
|||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|||
|- bgcolor="#ffffff" |
|||
|- |
|||
! bgcolor="# |
! bgcolor="#d0e7ff" align="center" |Al |
||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|[[RIE Etching Recipes|R2]] |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | Ru |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)|R1}} |
|||
|- |
|||
|[[ICP Etching Recipes#Al Etch .28Panasonic 2.29|R2]] |
|||
! bgcolor="#D0E7FF" align="center" | Ta |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | Ti |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|Ti Etch(Panasonic 1)}} |
|||
| A |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | Al<sub>2</sub>O<sub>3</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | Al<sub>2</sub>O<sub>3 (Sapphire)</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|Sapphire Etch(Panasonic 1)}} |
|||
| A |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Au |
|||
| |
| |
||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | AlGaAs |
|||
| |
|||
| |
|||
| |
|||
|{{rl|RIE Etching Recipes|AlGaAs Etch (RIE 5)}} |
|||
| |
|||
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}} |
|||
| |
|||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
| |
|||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | AlGaN |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | AlN |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
| |
|||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | CdZnTe |
|||
| |
|||
| {{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
| |
|||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | GaAs |
|||
| |
|||
| |
|||
| |
|||
| {{rl|RIE Etching Recipes|AlGaAs Etch (RIE 5)}} |
|||
| |
|||
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}} |
|||
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}} |
|||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | GaN |
|||
| |
|||
| |
|||
| |
|||
|{{rl|RIE Etching Recipes|RIE 5 (PlasmaTherm)|GaN Etch (RIE 5)}} |
|||
| |
|||
| {{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
|||
| |
|||
| {{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
|[[Other Dry Etching Recipes|R3]] |
|||
| |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Cr |
|||
| |
| |
||
|[[RIE Etching Recipes|R2]] |
|||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | GaSb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}} |
|||
|[[ICP Etching Recipes#Cr Etching (Panasonic 2)|R3]] |
|||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | HfO<sub>2</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | InGaAlAs |
|||
| |
|||
| {{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | InGaAsP |
|||
| |
|||
| {{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|R1 |
|||
|- bgcolor="#EEFFFF" |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Cu |
|||
| |
|||
| {{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|- |
|||
! bgcolor="#D0E7FF" align="center" | ITO |
|||
| |
|||
| {{rl|RIE Etching Recipes|ITO Etch (RIE 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
| |
|||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | Si |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|Si Etch (PlasmaTherm/Bosch Etch)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}} |
|||
| |
| |
||
| |
| |
||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ge |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Other Dry Etching Recipes|R2]] |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Mo |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- |
|- |
||
!Nb |
|||
! bgcolor="#D0E7FF" align="center" | SiC |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
|A |
||
|R1 |
|||
| {{rl|ICP Etching Recipes|SiC Etch(Panasonic 1)}} |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
|||
| |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ni |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|[[Other Dry Etching Recipes|R3]] |
|||
|- |
|- |
||
!Os |
|||
! bgcolor="#D0E7FF" align="center" | SiN |
|||
| |
|||
| |
|||
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}} |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|SINxEtch(Panasonic 1)}} |
|||
| {{rl|ICP Etching Recipes|SINxEtch(Panasonic 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | SiO<sub>2</sub> |
|||
| |
|||
| |
|||
| {{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}} |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|SIO2Etch(Panasonic 1)}} |
|||
| {{rl|ICP Etching Recipes|SIO2Etch(Panasonic 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|A |
|||
| {{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}} |
|||
|R1 |
|||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | SiOxNy |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Pt |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Other Dry Etching Recipes|R3]] |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ru |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Si |
|||
| |
|||
| |
|||
|[[ICP Etching Recipes#High Rate Bosch Etch (DSEIII)|R6]], [[ICP Etching Recipes#Silicon: Single-Step, Low Etch Rate, Smooth Sidewall Process (DSEIII)|R3]] |
|||
|[[ICP Etching Recipes#Si Etch Recipes (Fluorine ICP Etcher)|R6]] |
|||
| |
|||
| |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Other Dry Etching Recipes|R3]] |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ta |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Ti |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}} |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |W |
|||
| |
|||
| |
|||
| |
|||
|[[ICP Etching Recipes#W Etching (Fluorine ICP Etcher)|R3]] |
|||
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}} |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- |
|- |
||
!TiW |
|||
! bgcolor="#D0E7FF" align="center" | Ta<sub>2</sub>O<sub>5</sub> |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
|R3 |
||
| |
| |
||
| |
|R1 |
||
| |
|||
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A] |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}} |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |AlGaAs |
|||
| |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}} |
|||
| |
|||
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |AlGaN |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R2]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |AlN |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|R1 |
|||
|- |
|- |
||
!BCB |
|||
! bgcolor="#D0E7FF" align="center" | TiN |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | TiO<sub>2</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
|A |
|||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | W-TiW |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| {{rl|ICP Etching Recipes|W-TiW Etch(Panasonic 1)}} |
|||
| A |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
|- bgcolor="#EEFFFF" |
|||
! bgcolor="#D0E7FF" align="center" | ZnO<sub>2</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |CdZnTe |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |GaAs |
|||
| |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}} |
|||
|[[ICP Etching Recipes#GaAs Etch .28Panasonic 2.29|R6]] |
|||
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |GaN |
|||
| |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
|||
|R1 |
|||
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R6]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |GaSb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|R1 |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- |
|- |
||
!Hf |
|||
! bgcolor="#D0E7FF" align="center" | ZnS |
|||
| |
|||
| {{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
| |
|||
| |
|||
| |
|||
| |
|||
|R2 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |InGaAsP |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |InP |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|R1 |
|||
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R6]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Other Dry Etching Recipes|R3]] |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |ITO |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- |
|- |
||
!LiNbO3 |
|||
! bgcolor="#D0E7FF" align="center" | ZnSe |
|||
| |
|||
| {{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
|||
| |
| |
||
| |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
!Photoresist & Organics |
|||
| |
|||
|[[RIE Etching Recipes#Photoresist and ARC (RIE 5)|R3]] |
|||
| |
|||
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
|||
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R3] |
|||
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]] |
|||
| |
|||
|R3 |
|||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- |
|- |
||
!ARC (Anti Reflective Coating) |
|||
! bgcolor="#D0E7FF" align="center" | ZrO<sub>2</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |SiC |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}} |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |SiN |
|||
| |
|||
| |
|||
| |
|||
|[[ICP Etching Recipes#Si3N4 Etching .28Fluorine ICP Etcher.29|R3]] |
|||
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
|||
|[[ICP Etching Recipes#SiNx Etching .28Panasonic 2.29|R3]] |
|||
| |
|||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
|||
| |
|||
| |
|||
|[[ICP Etching Recipes#SiO2 Etch (DSEiii)|R3]] |
|||
|[[ICP Etching Recipes#SiO2 Etch Recipes (Fluorine ICP Etcher)|R6]] |
|||
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
|||
|[[ICP Etching Recipes#SiO2 Etching .28Panasonic 2.29|R6]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Other Dry Etching Recipes|R3]] |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |SiOxNy |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- |
|- |
||
!SU8 |
|||
! bgcolor="#D0E7FF" align="center" | '''Material''' |
|||
| |
|||
| bgcolor="#DAF1FF" | [[RIE 1 (Custom)|RIE 1<br>(Retired)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]] |
|||
|A |
|||
| bgcolor="#DAF1FF" | [[ICP_Etching_Recipes#Si_Deep_RIE_.28PlasmaTherm.2FBosch_Etch.29|Si Deep RIE<br>(PlasmaTherm/Bosch Etch)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic E626I)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic E640)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]] |
|||
| |
|||
| bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]] |
|||
|- bgcolor="#eeffff" |
|||
| bgcolor="#DAF1FF" | [[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]] |
|||
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|A |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |TiN |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |ZnS |
|||
|[[RIE Etching Recipes|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |ZnSe |
|||
|[[RIE Etching Recipes|R2]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#ffffff" |
|||
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|R1 |
|||
|- bgcolor="#eeffff" |
|||
! bgcolor="#d0e7ff" align="center" |'''Material''' |
|||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
|||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
|||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
|||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
|||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
|||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]] |
|||
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
|||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
|||
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
|||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
|||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]] |
|||
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]] |
|||
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]] |
|||
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]] |
|||
|} |
|} |
||
===Process Ranking Table=== |
|||
Processes in the table above are ranked by their "''Process Maturity Level''" as follows: |
|||
{| class="wikitable" |
|||
!Process Level |
|||
! colspan="11" |Description of Process Level Ranking |
|||
|- |
|||
|A |
|||
| colspan="11" |Process '''A'''llowed and materials available but never done |
|||
|- |
|||
|R1 |
|||
| colspan="11" |Process has been ran at least once |
|||
|- |
|||
|R2 |
|||
| colspan="11" |Process has been ran and procedure is documented |
|||
|- |
|||
|R3 |
|||
| colspan="11" |Process has been ran, procedure is documented, and data is available |
|||
|- |
|||
|R4 |
|||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''no''' in-Situ control available |
|||
|- |
|||
|R5 |
|||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' in-Situ control available |
|||
|- |
|||
|R6 |
|||
| colspan="11" |Process has a documented procedure and control charts/limits available. Controlled process. |
|||
|} |
|||
[[Category:Processing]] |
[[Category:Processing]] |
||
Latest revision as of 22:16, 23 September 2026
Process Control Data
See above linked page for process control data (dep rate/stress etc. over time), for a selection of often-used dry etches
Dry Etching Tools/Materials Table
Process Maturity Ranking
R6- most mature process with regular calibrations recorded on SPC charts.- …
R1- least mature - only run once ever.
The Key/Legend for this table's A...R6 values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
| Process Level | Description of Process Level Ranking | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| A | Process Allowed and materials available but never done | ||||||||||
| R1 | Process has been ran at least once | ||||||||||
| R2 | Process has been ran and procedure is documented | ||||||||||
| R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
| R4 | Process has a documented procedure with regular (≥4x per year) data no in-Situ control available | ||||||||||
| R5 | Process has a documented procedure with regular (≥4x per year) data and in-Situ control available | ||||||||||