There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning). |
|||
The wafers used for process calibration are ordered from SVM. These are low particle count 4" Si wafers (particle count<100). The wafers are scanned before and after deposition. They are not re-used. Handling the wafers is important and each step could contribute in adding new particles. |
|||
=== Standard Si3N4 (Silicon-Nitride) Deposition === |
|||
== SiN @250C == |
|||
| ⚫ | |||
# Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes. |
|||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
# Load the deposition recipe, and run it. |
|||
# Wait for deposition to be finished. Unload the wafer. |
|||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
== |
==== SiN Deposition ==== |
||
# Log in to PECVD #1 |
# Log in to PECVD #1 |
||
| ⚫ | |||
# Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes. |
|||
| ⚫ | |||
| ⚫ | |||
# |
# Deposition |
||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
#* Load the deposition recipe (SiN@250C), and run it. Deposition time is variable. Get the rate from [https://wiki.nanotech.ucsb.edu/wiki/PECVD_Recipes#PECVD_1_.28PlasmaTherm_790.29 historical data]. |
|||
| ⚫ | |||
#* Unload the wafer. |
|||
| ⚫ | |||
| ⚫ | |||
# Load the deposition recipe, and run it. |
|||
#* Wipe sidewall first with DI water, followed by IPA. |
|||
# Wait for deposition to be finished. Unload the wafer. |
|||
#* Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning. |
|||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
=== Standard Oxide, SiO2 (Silicon Dioxide) Deposition === |
|||
==== SiO2 Deposition ==== |
|||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
#* Load the deposition recipe( SiO2@250C), and run it. Deposition time is variable. Get the rate from [[PECVD Recipes#PECVD 1 .28PlasmaTherm 790.29|historical data]]. |
|||
#* Unload the wafer. |
|||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
Latest revision as of 20:16, 10 December 2020
There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning).
Standard Si3N4 (Silicon-Nitride) Deposition
SiN Deposition
- Log in to PECVD #1
- Seasoning
- Load the seasoning recipe (SiN seasoning), and run it. The goal of this step is to coat chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (SiN@250C), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning.
- Log out
Standard Oxide, SiO2 (Silicon Dioxide) Deposition
SiO2 Deposition
- Log in to PECVD #1
- Seasoning
- Load the seasoning recipe( SiO2 seasoning), and run it. The goal of this step is to coat chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substarte (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe( SiO2@250C), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load for cleaning recipe (CF4/O2). Edit the recipe and enter required time for cleaning.
- Log out