There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning). |
|||
The wafers used for process calibration are ordered from SVM. These are low particle count 4" Si wafers (particle count<100). The wafers are scanned before and after deposition. They are not re-used. Handling the wafers is important and each step could contribute in adding new particles.The section bellow describes how to run standard recipes for SiN a,d SiO2 at 250C. |
|||
=== Standard Si3N4 (Silicon-Nitride) Deposition === |
|||
| ⚫ | |||
| ⚫ | |||
# Log in to PECVD #1 |
# Log in to PECVD #1 |
||
# Seasoning |
# Seasoning |
||
| Line 8: | Line 10: | ||
#* Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving. |
#* Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving. |
||
#* Pump down. |
#* Pump down. |
||
#* Load the deposition recipe (SiN@250C), and run it. |
#* Load the deposition recipe (SiN@250C), and run it. Deposition time is variable. Get the rate from [https://wiki.nanotech.ucsb.edu/wiki/PECVD_Recipes#PECVD_1_.28PlasmaTherm_790.29 historical data]. |
||
#* Unload the wafer. |
#* Unload the wafer. |
||
# Cleaning |
# Cleaning |
||
#* Wipe sidewall first with DI water, followed by IPA. |
#* Wipe sidewall first with DI water, followed by IPA. |
||
#* Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning. |
#* Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning. |
||
#* Log out |
#* Log out |
||
=== Standard Oxide, SiO2 (Silicon Dioxide) Deposition === |
|||
| ⚫ | |||
| ⚫ | |||
#Log in to PECVD #1 |
#Log in to PECVD #1 |
||
# Seasoning |
# Seasoning |
||
| Line 22: | Line 26: | ||
#* Vent the chamber and load the substarte (place it in the center of platen). You can place small pieces around the wafer to protect it from moving. |
#* Vent the chamber and load the substarte (place it in the center of platen). You can place small pieces around the wafer to protect it from moving. |
||
#* Pump down. |
#* Pump down. |
||
#* Load the deposition recipe( SiO2@250C), and run it. |
#* Load the deposition recipe( SiO2@250C), and run it. Deposition time is variable. Get the rate from [[PECVD Recipes#PECVD 1 .28PlasmaTherm 790.29|historical data]]. |
||
#* Unload the wafer. |
#* Unload the wafer. |
||
# Cleaning |
# Cleaning |
||
Latest revision as of 20:16, 10 December 2020
There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning).
Standard Si3N4 (Silicon-Nitride) Deposition
SiN Deposition
- Log in to PECVD #1
- Seasoning
- Load the seasoning recipe (SiN seasoning), and run it. The goal of this step is to coat chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (SiN@250C), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning.
- Log out
Standard Oxide, SiO2 (Silicon Dioxide) Deposition
SiO2 Deposition
- Log in to PECVD #1
- Seasoning
- Load the seasoning recipe( SiO2 seasoning), and run it. The goal of this step is to coat chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substarte (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe( SiO2@250C), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load for cleaning recipe (CF4/O2). Edit the recipe and enter required time for cleaning.
- Log out