Thermal Evap 2 (Solder): Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(fixed link to recipes, removed duplicate link)
 
(11 intermediate revisions by 3 users not shown)
Line 1: Line 1:
{{tool|{{PAGENAME}}
{{tool2|{{PAGENAME}}
|picture=Thermal2.jpg
|picture=Thermal2.jpg
|type = Vacuum Deposition
|type = Vacuum Deposition
|super= Don Freeborn
|super= Michael Barreraz
|super2= Don Freeborn
|location=Bay 3
|location=Bay 3
|description = ?
|description = ?
Line 12: Line 13:
== About ==
== About ==
Thermal evaporator #2 is the designated "Solder" evaporator. The tool is used primarily for solder materials including Gold, Indium and Tin.
Thermal evaporator #2 is the designated "Solder" evaporator. The tool is used primarily for solder materials including Gold, Indium and Tin. See the Recipes section below for other materials used.


Use this tool for materials with low melting temperatures, or for materials that have a high risk of contamination in the e-beam evaporators.
Use this tool for materials with low melting temperatures, or for materials that have a high risk of contamination in the e-beam evaporators.
Line 21: Line 22:
==Documentation==
==Documentation==
*[//wiki.nanotech.ucsb.edu/w/images/b/b3/Thermal_Evaporator2.pdf Operating Instructions]
*[//wiki.nanotech.ucsb.edu/w/images/b/b3/Thermal_Evaporator2.pdf Operating Instructions]
*[https://wiki.nanofab.ucsb.edu/w/images/1/17/Thermal_Evaporator2-Normal_Fixture-_Indium_Deposition.pdf Using Normal Fixture]
*[https://wiki.nanofab.ucsb.edu/w/images/d/d1/Thermal_Evaprator2-Cold_Fixture-Indium_Deposition.pdf Using Cold Fixture]
*[https://wiki.nanofab.ucsb.edu/w/images/7/74/Thermal_Evap_2_pump_down_procedure-New-_5-29-25.pdf Temp Pump Down SOP as of 5-29-25]


== Recipes ==
== Recipes ==
* [[Thermal Evaporation Recipes#Thermal Evaporator 2|Recipes > Thermal Evaporation Recipes > Thermal Evaporator 2]]
* [[Thermal Evaporation Recipes#Thermal Evaporator 2|Recipes > Thermal Evaporation Recipes > Thermal Evaporator 2]]
** ''Visit this page for the materials tables and evaporation parameters.''
** ''Visit this page for the materials table and evaporation parameters for all materials available.''
== Plot ==
* [https://wiki.nanofab.ucsb.edu/w/images/b/bb/Thermal_Evaporator2-Plot.png Plot for Indium Deposition]

Latest revision as of 16:29, 29 May 2025

Thermal Evap 2 (Solder)
Thermal2.jpg
Location Bay 3
Tool Type Vacuum Deposition
Manufacturer Custom
Description ?

Primary Supervisor Michael Barreraz
(805) 893-4147
mikebarreraz@ece.ucsb.edu

Secondary Supervisor

Don Freeborn


Recipes Vacuum Deposition Recipes

SignupMonkey: Sign up for this tool


About

Thermal evaporator #2 is the designated "Solder" evaporator. The tool is used primarily for solder materials including Gold, Indium and Tin. See the Recipes section below for other materials used.

Use this tool for materials with low melting temperatures, or for materials that have a high risk of contamination in the e-beam evaporators.

Detailed Specifications

Wafers up to 12" can be mounted.

Documentation

Recipes

Plot