PECVD Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Biljana (talk | contribs)
Biljana (talk | contribs)
→Si3N4 [ICP-PECVD]: SiN parameters
 
(137 intermediate revisions by 2 users not shown)
Line 1: Line 1:
{{recipes|Vacuum Deposition}}
{{recipes|Vacuum Deposition}}

=[[PECVD 1 (PlasmaTherm 790)]]=
=[[PECVD 1 (PlasmaTherm 790)]]=
==== Historical Particulate Data ====


*[https://docs.google.com/spreadsheets/d/1a0XrY6HuJ6L9niThZYI-u4XH69Hnbe3jkm1qKmrR8Rg/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2015]
===[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1270764394 PECVD 1 Process Control Plots] - Plots of all process control data===
*[https://docs.google.com/spreadsheets/d/1ZfkspbCQZmdThC8qB4XyjsyPAzrMF1QbHSMFmH6xSo4/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2016]
*[https://docs.google.com/spreadsheets/d/1YNiof68Veeh08s_NtG5aCWUXW7GWDDU00HAimV_l8_g/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2017]
*[https://docs.google.com/spreadsheets/d/1VN551M2oXGWX306HDLQXvZIp3kgxEvWffQqMqnc8ISk/edit#gid=sharing Particulates in PECVD#1 films 2017]
*[https://docs.google.com/spreadsheets/d/11c0gQHnattIjVO95aBqiL-zL4DInRFihV-YB54xLT40/edit#gid=sharing Particulates in PECVD#1 films 2018]
*[https://docs.google.com/spreadsheets/d/1ct-SSCRxf81W0jupCWzh81n0DBwPv6mwKFMzuWu_0TI/edit#gid=sharing Particulates in PECVD#1 films 2019]
*[https://docs.google.com/spreadsheets/d/1yks0OgH8rpbYjin_Qr8vpPg8jBiZQRs_PKfyfo-Rqg0/edit#gid=sharing Particulates in PECVD#1 films 2020]


==SiN deposition (PECVD #1)==
==SiO<sub>2</sub> deposition (PECVD #1)==


*[https://docs.google.com/spreadsheets/d/1uqpg3sirsRbXdTFlxZ6_k3t0ovP0MtpFtICjpH0-prs/edit?usp= Si3N4 Standard Recipe]
*[https://docs.google.com/spreadsheets/d/1wloq6HJw5RQIvmeKcBn3xvE_917R6jF_K-btCHjsiIM/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
*[https://docs.google.com/spreadsheets/d/10ccfgCf5O0JM6L9J5XDz-gWVQz9P24VU/edit#gid= Si3N4 Recipe parameters]
==== Historical Data ====


*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
===== Thin-Film Properties =====
**Lists film data, such as dep rate, stress, particle count, refractive index etc.


=== Old Data ===
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN 100nm Data 2014]
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.231.29 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier
*[https://docs.google.com/spreadsheets/d/1phx1WficlUEg0xSahaAq4zrRk6m9Eb0ausO8wcAmXqs/edit#gid=sharing SiN 100nm Data 2015]
*[https://docs.google.com/spreadsheets/d/1VNSNTqnbE4SFk0HyhBAy3GJzi0jRQEs8cgk1v2_Uam8/edit#gid=sharing SiN 100nm Data 2016]
*[https://docs.google.com/spreadsheets/d/1TG1X2wpl2fWaHEtAHtpZFBVSCk1BQeGJQ8LA2M2qBJ0/edit#gid=sharing SiN 100nm Data 2017]
*[https://docs.google.com/spreadsheets/d/1UlyvPcXUBQ5R2JwjKOjELvtCJaTElVhJHfzgjyaRd2A/edit#gid=sharing SiN 300nm Data 2017]
*[https://docs.google.com/spreadsheets/d/1pAoTCaNSf0uZMyiQ2qKFd0s_e4e53P9Z1jUwtmTnlLk/edit#gid=sharing SiN 300nm Data 2018]
*[https://docs.google.com/spreadsheets/d/1Pnw8eEaQ0rGblRYl6LeIm6wrh1hgeyjnHEbA4BzV8JM/edit#gid=sharing SiN 300nm Data 2019]
*[https://docs.google.com/spreadsheets/d/1N_1Kk6J-wA4nlHpFg5EMDZNHR1kLDo_fr_Dvc6osSr4/edit#gid=sharing SiN 300nm Data 2020]


===== Uniformity Data =====
==SiN deposition (PECVD #1)==


*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 100 nm Thickness uniformity 2014]
*[https://docs.google.com/spreadsheets/d/1-pET1Eojooso5UHk90W-5uYByDDdrCyRnggqewxTmVg/edit#gid=sharing SiN 100 nm Thickness uniformity 2015]
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=98787450 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://docs.google.com/spreadsheets/d/1V_-KzsdR-2tSnJGtUdQWokmnNIY949t0vdQOp7RfCgc/edit#gid=sharing SiN 100 nm Thickness uniformity 2016]
*[https://docs.google.com/spreadsheets/d/1tM-a4VBEqpxr2G8PGGLTbsR6BQBmvqXNRBw0mikAUS0/edit#gid=sharing SiN 100 nm Thickness uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1Z83RCH5cAUfViO6vv6hAatcLVWZ95ex4nDdfffm9I7s/edit#gid=sharing SiN 300nm Thickness uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1b4EQZdRtVbqNwGBrItoG5-tz6RIzlsvBiCFR6ZXfylw/edit#gid=sharing SiN 300nm Thickness uniformity 2018]
*[https://docs.google.com/spreadsheets/d/1-OiaH8frAzJzHKfbYTJP808ddzk1Wsv_CixDzG-sSfo/edit#gid=sharing SiN 300nm Thickness uniformity 2019]
*[https://docs.google.com/spreadsheets/d/1eP6U2WJetu2wDB6wemkMPFG0JYx33I3Z3liihwae8Oo/edit#gid=sharing SiN 300nm Thickness uniformity 2020]


=== Old Data ===
==SiO<sub>2</sub> deposition (PECVD #1)==
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.231.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier


==Low Stress Si<sub>3</sub>N<sub>4</sub> (PECVD#1)==
*[https://docs.google.com/spreadsheets/d/1uqpg3sirsRbXdTFlxZ6_k3t0ovP0MtpFtICjpH0-prs/edit#gid= SiO2 Standard Recipe]
*[https://docs.google.com/spreadsheets/d/10ccfgCf5O0JM6L9J5XDz-gWVQz9P24VU/edit#gid= SiO2 Recipe parameters]


*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
==== Historical Data ====
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#Low-Stress_SiN_-_LS-SiN_.28PECVD.231.29 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - 2021-10 and earlier


:[[File:PECVD1 SiN Stress vs. N2 plot.jpg|alt=plot of SiN stress and Refractive Index vs. N2 flow. |none|thumb|414x414px|Example of Si<sub>3</sub>N<sub>4</sub> modified stress via. varying N<sub>2</sub> flow.  Refractive index is relatively constant (one outlier), and stress varies continuously from tensile to compressive.  ([[Demis D. John]] 2011, [https://engineering.ucsb.edu/people/daniel-blumenthal Blumenthal Group])]]
===== Thin-Film Properties =====


==SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1)==
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEw0bjFEdTF2SUhRa25Ca0d0SzBha3c&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Data 2014]
*[https://docs.google.com/spreadsheets/d/1JWNUcH8l90xif-0BhYKJee9nXxE4hnvvp6N2NtZLYXY/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2015]
*[https://docs.google.com/spreadsheets/d/1F2pfsVnbUgaE9tsm8HZMlY6cyt-nhui0IpvGc6udhDU/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2016]
*[https://docs.google.com/spreadsheets/d/1MblK5Zr5Skfw0s9Hdhqr_cCwN-nCgM-ofZnsAyvVRq8/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2017]
*[https://docs.google.com/spreadsheets/d/15SocIqWQvBKSvT5oCWoZAURLaaqb9KosxCN2rueZQN8/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2017]
*[https://docs.google.com/spreadsheets/d/1DdjIRGsfJ7WCrxQoGpmzkjLGJhpBTFNYLFmmHcNjAjk/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2018]
*[https://docs.google.com/spreadsheets/d/1QbhukSuVNueT067IVEpweSlD4B7GQecf-tfQFQeV6Xs/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2019]
*[https://docs.google.com/spreadsheets/d/1OwyhfFPDH-XLPczA8cKoBPnujq9oNukaWkHq0KoFS40/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2020]


*[https://wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]
==== Uniformity Data ====
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] - ''Lists film data, such as dep rate, stress, particle count, refractive index etc.''
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]


==Standard Cleaning Procedure (PECVD #1)==
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDQ3VEtZQVRpdVdlbGtIZHpTNmFzNmc&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Thickness uniformity 2014]
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.
*[https://docs.google.com/spreadsheets/d/1NQy-ADou6f2NBU-9jZG8KME1lOz0X5mh6HZV9_jPGes/edit#gid=sharing SiO<sub>2</sub> 100 nm Thickness uniformity 2015]
*[https://docs.google.com/spreadsheets/d/1WUCm_dWpxKTjfFf1rNfLuxvwMxsyCYON_OZ3gb50L_s/edit#gid=sharing SiO<sub>2</sub> 100 nmThickness uniformity 2016]
*[https://docs.google.com/spreadsheets/d/1dpC_AkPD-etIH6fVuQqLfd4UMNQCEtcqhvmBpwbEncE/edit#gid=sharing SiO<sub>2</sub> 100nm Thickness uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1Fa8mZIBIeJwvCwUbJ-28VcvVYj8rshhuDuXsYxA-cD8/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1YB_9USpuXGpIdSW2gNsptu5nSrLWAGsYu0SWoYEy0aQ/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2018]
*[https://docs.google.com/spreadsheets/d/1FatUAEegWuDRzVa47L1_cqgRs0AZ_Fao9jpwz5sfln0/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2019]
*[https://docs.google.com/spreadsheets/d/1cUIEs2_RYK741CAaVVlfzqTEOqlPHQ9MnhgJ6fdTWMc/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2020]


The clean is done in two steps:
== Low-Stress SiN - LS-SiN (PECVD#1) ==


#'''Wet cleaning''' (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
*[//wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf LS SiN Standard Recipe]
#Load the recipe for plasma cleaning "'''''CF4/O2 Clean'''''" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.
*[https://docs.google.com/spreadsheets/d/1Joz0az9TGZWQc4CiMQJZzLBbNFbx_hH2Oc0B4NNJmYk/edit#gid=sharing LS SiN Data 2014]
*[https://docs.google.com/spreadsheets/d/1xIzc2CufRYNSfAtsOXpw3IzHreeu42BWrLBV0kzP6kA/edit#gid=sharing LS SiN 1000A Thickness uniformity 2014]


{| class="wikitable"
== SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1) ==
|+Table of Cleaning Times
!Film Dep'd
!Cleaning Time
|-
|SiO<sub>2</sub>
|1 min clean for every 1 min dep
|-
|Si<sub>3</sub>N<sub>4</sub>
|1 min clean for every 7 min dep
|-
|SiOxNy
|Same as SiO<sub>2</sub>
|-
|a-Si
|Same time as Si<sub>3</sub>N<sub>4</sub>
|}


*[//wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]
===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]===
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that '''it will pop up a window for the cleaning time''' upon running the recipe - you do not need to edit the recipe before running it.
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]

== Cleaning Recipes (PECVD #1) ==
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
# Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
# Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.

=== [//wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe: "CF4/O2 Clean"] ===
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will '''pop up a window for the cleaning time upon running the recipe''' - you do not need to edit the recipe before running it.


=[[PECVD 2 (Advanced Vacuum)]]=
=[[PECVD 2 (Advanced Vacuum)]]=


===[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=272916741 PECVD 2 Process Control Plots] - Plots of all process control data===
==== Historical Particulate Data ====


==SiO<sub>2</sub> deposition (PECVD #2)==
*[https://docs.google.com/spreadsheets/d/1kj0SWxRpnPRoGld8k3sW-3yK1iPm3buTkvlJSN5YPV4/edit#gid=sharing Particulates (Gain4) in PECVD#2 2015]
*[https://docs.google.com/spreadsheets/d/1xpk9tJrE68NIJ_1yIym0xBxd4fnzHHBHdkhFehruO3E/edit#gid=sharing Particulates (Gain4) in PECVD#2 2016]
*[https://docs.google.com/spreadsheets/d/1ICgt-fgTvNPbE_65x5jUsqy8JjHVv5WUvmE7g7VUbsI/edit#gid=sharing Particulates (Gain4) in PECVD#2 2017]


*[https://docs.google.com/spreadsheets/d/1yPAPP24z3RcRRi-HqEp3GJN4JM8Ec8SFJwZ-OYGG2HU/edit#gid=sharing Particulates in PECVD#2 films 2017]
*[https://docs.google.com/spreadsheets/d/1cYK-k669vf8YO2q2YCGa3gTdaDI3I3M-a9KR5RDlZWY/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD SiO2 v2''"
*[https://docs.google.com/spreadsheets/d/1aU6fTyQ5MlGD4uCa9gepG5rLJzW3wlkOWSKEl_w_Ye4/edit#gid=sharing Particulates in PECVD#2 films 2018]
**[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''STD SiO2''"
*[https://docs.google.com/spreadsheets/d/1OPZXe8g3H0wywIrPFel3nSZ5iyPs2mVIYUSVKfTtMDg/edit#gid=sharing Particulates in PECVD#2 films 2019]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=1313651154 SiO<sub>2</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://docs.google.com/spreadsheets/d/1Y9lomsf7bDojeXoAsEG7xvypx_sw_atpmPwB9xtK1Zk/edit#gid=sharing Particulates in PECVD#2 films 2020]
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.232.29 SiO<sub>2</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021


==SiO<sub>2</sub> deposition (PECVD #2)==
*SiO<sub>2</sub> deposition rate at 150C is 35nm/min


==== Standard Recipe ====
==SiN deposition (PECVD #2)==


*[https://docs.google.com/spreadsheets/d/1vgWUtpCWC_TFffU9kuR3wqvjryiNA5OV/edit#gid= STD SiO2 Recipe Parameters]
*[https://docs.google.com/spreadsheets/d/1JBXEfRGemFJK81RkHfxS0cTucb3viUL7hMGzmKRD5uU/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD Si3N4 v3''"
*[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= STD SiO2 Recipe]
**[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "''Nitride2''"
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=773875841 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.232.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021


==Low-Stress SiN deposition (PECVD #2)==
==== Historical Data ====
''Low-Stress Silicon Nitride, Si<sub>3</sub>N<sub>4</sub> (< ±100 MPa)''


*[https://docs.google.com/spreadsheets/d/19VQ6ytYbZ5SsAiXzgWqwlyJUqgjWb8x_eyv7L8DvtwM/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] New Standard Recipe</nowiki>] - "''STD LS-Si3N4 v4''"
===== Thin-Film Properties =====


**[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Old Standard Recipe</nowiki>] - "'' Old LSNitride2 recipe ''"
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]
*[https://docs.google.com/spreadsheets/d/1d5boeJRWWgMqvQe6nVM7m8s3KAcS4Yp2L5CEU9svkX4/edit#gid=sharing Oxide Data 2015]
*[https://docs.google.com/spreadsheets/d/1XQRcTJdw9AIMPAUsH0n9Ic9Fe1_xGDSvAxD4gVc9FBw/edit#gid=sharing Oxide data 2016]
*[https://docs.google.com/spreadsheets/d/1vcaHwraMGNHuRxgWwGp78EJf4T3Jk182wxoCz_neuck/edit#gid=sharing Oxide Data 2017]
*[https://docs.google.com/spreadsheets/d/1VI-sUmaqois0NsCvf2kQmPfRRa03MjBzl779hmmLtP4/edit#gid=sharing Oxide Data 2018]
*[https://docs.google.com/spreadsheets/d/1oWnQ3D6oknKWU2bohvSrN85rlEZgQN3YP_ZJ4i8u7do/edit#gid=sharing Oxide Data 2019]
*[https://docs.google.com/spreadsheets/d/1Z9UMgaQC2PiLLrMk04mpKWkJLa1L_WFMAm5079eKxI0/edit#gid=sharing Oxide Data 2020]


*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=203400760 Plots of Low-Stress Si<sub>3</sub>N<sub>4</sub> Process Control Data]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[[Old Deposition Data - 2021-12-15#Low-Stress SiN deposition .28PECVD .232.29|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data - Before Oct. 2021</nowiki>]]
*:''Old Versions of the recipe:''
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]''
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018]''


===Low-Stress SiN 3xTime (PECVD #2)===
===== Uniformity Data =====
''This Low-Stress SiN recipe is more stable over time (months), because each step is 3x longer (so each compressive/tensile layer is thicker), making it less susceptible to RF ignition delays as the grounding strap is etched over time. – 2024-09 [[Demis D. John|Demis]] & [[Biljana Stamenic|Biljana]]''


*Recipe: "''[https://docs.google.com/spreadsheets/d/1OQp_sux5YEgpcyH3sf0JCwTOhvoi_LSYKOUMRR4Umh4?usp=drive_fs STD LS-Si3N4 3xTime v1]"''
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness Uniformity 2014]
*[https://docs.google.com/spreadsheets/d/16pZHcGwesXB1mMPwntOudBIlPvRh6A6DI37DEwyYfPw/edit#gid=sharing Oxide Thickness Uniformity 2015]
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?usp=sharing Process Control Data]: Lists film data, such as dep rate, stress, particle count, refractive index etc.
*[https://docs.google.com/spreadsheets/d/10OEuANVNmHqWvx-92zibechIrHK5kgqSK4B_O_O3-YI/edit#gid=sharing Oxide Thickness Uniformity 2016]
*[https://docs.google.com/spreadsheets/d/15aKkk-fIojIDgQfsVlB3lhex-U3Q0edVdNCkzoGBo1Q/edit?gid=974005628#gid=974005628 Process Control Charts/Plots]: Calibration control limits versus date
*[https://docs.google.com/spreadsheets/d/19JjJYdFNFzO685Hp9hODVRFAYF5bP3IEYGTRGQjqLN4/edit#gid=sharing Oxide Thickness Uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2018]
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2019]
*[https://docs.google.com/spreadsheets/d/1Z9UMgaQC2PiLLrMk04mpKWkJLa1L_WFMAm5079eKxI0/edit#gid=sharing Oxide Thickness Uniformity 2020]


==SiN deposition (PECVD #2)==
==Amorphous-Si deposition (PECVD #2)==


*[[PECVD-2 - a-Si Recipe and Dep process (2025)|a-Si Recipe and Dep process]] 2025-11
==== Standard Recipe ====
**''Developed by Ryan Hersey & Skyler Palatnik, Group of Prof. Max Millar-Blanchaer''
*[https://wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe] (2013-09, Ning Cao)
*[https://wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Film - Characterization and Stress] - DOE/recipe variations


==Standard Cleaning Procedure (PECVD #2)==
*[//wiki.nanotech.ucsb.edu/wiki/images/4/4c/SiNx_Films_by_PECVD2.pdf SiNx Film Stress vs LF and HF Duration Time, and Gas Flowing-rate]
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
*[https://docs.google.com/spreadsheets/d/1Oegk0aFFCuz9wQHDN2Kdz0NFo9_wuEVW/edit?dls=true#gid= STD Nitride2 Recipe Parameters]


#If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
*[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= STD Nitride2 Recipe]
#Load the recipe for cleaning "STD CF<sub>4</sub>/O<sub>2</sub> Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.


===[https://wiki.nanofab.ucsb.edu/wiki/File:STD_CF4-O2_Clean_PECVD2.jpg Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"]===
==== Historical Data ====
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


===== Thin-Film Properties =====


'''Clean Times (PECVD#2''')
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]
{| class="wikitable"
*[https://docs.google.com/spreadsheets/d/1SkYqOwgjUyMaFBPhuTjMvBTXu0KdQFNmITryF_OVi8o/edit#gid=sharing Nitride2 Data 2015]
!Film Deposited
*[https://docs.google.com/spreadsheets/d/1HJszgZyEZR9ZsiJpQM6pdsoQ6pWwI6brXasdmfDRoBQ/edit#gid=sharing Nitride2 Data 2016]
!Cleaning Time (Dry)
*[https://docs.google.com/spreadsheets/d/1f3JBEnr7lf0yIMlzlOYKv_bXlIDyXt8vec_rSVJIoOk/edit#gid=sharing Nitride2 Data 2017]
|-
*[https://docs.google.com/spreadsheets/d/1OO0ewGSqYSzL3lj8fXkgckTkBGQRliD6sBc02IW7wZY/edit#gid=sharing Nitride2 Data 2018]
|SiO<sub>2</sub>
*[https://docs.google.com/spreadsheets/d/1Zi8CRspd3LTDdNRRCneE0--bVohWvZbV_kSHo04s0oI/edit#gid=sharing Nitride2 Data 2019]
|1min. clean for every 1min. deposition
*[https://docs.google.com/spreadsheets/d/15UAXRIOO_aHvGCyTzV0dSZKdq0TUqPxVxuDlva2B1BI/edit#gid=sharing Nitride2 Data 2020]
|-
|Si<sub>3</sub>N<sub>4</sub>
|1min. clean for every 7min. of deposition
|-
|a-Si
|2 min clean for every 1min of deposition
|-
|a-Si (max 60min dep before breaking it up and cleaning the chamber)
|Wet Clean the Upper Lid/Chamber
DI water then Isopropyl Alcohol on chamber wall & portholes
|-
|Other films:(max 60min long dep. in one single run)
|If > 29min total dep time
(Season + Dep)


Wet Clean the Upper Lid/Chamber


DI water then Isopropyl Alcohol on chamber wall & portholes
|}


=[[ICP-PECVD (Unaxis VLR)]]=
===== Uniformity Data =====
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the [[ICP-PECVD (Unaxis VLR)#Documentation|new procedures]] to ensure low particle counts in the chamber.


The system currently has '''Deuterated Silane (SiD<sub>4</sub>)''' installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness Uniformity 2014]
*[https://docs.google.com/spreadsheets/d/14_dYQu3z31fF_oxsUUX8BmDucgv6B07xB3_zqP0HmvM/edit#gid=sharing Nitride2 Thickness Uniformity 2015]
*[https://docs.google.com/spreadsheets/d/1qBHs7uALM2OdE-yXOq4uZk6aUQEjZRjG1C6RcMEf0sk/edit#gid=sharing Nitride2 Thickness Uniformity 2016]
*[https://docs.google.com/spreadsheets/d/1WJcYzHUjLrWpys_i-Q96FN_lBDBufpXZKZVEX_gri_Q/edit#gid=sharing Nitride2 Thickness Uniformity 2017]
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2018]
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2019]
*[https://docs.google.com/spreadsheets/d/16nlLjk_kctE6YKQBJbq0SotP80tybdSdJ0hvxbeohE0/edit#gid=sharing Nitride2 Thickness Uniformity 2020]


==Process Control Data (Unaxis ICP-PECVD)==
==Low-Stress SiN deposition (PECVD #2)==
''Regularly-run depositions and measurements of film properties over time - executed by [https://nanofab.ucsb.edu/workforce NanoFab Interns].''
''Low-Stress SilIcon Nitride (< 100 MPa)''
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Process Control Plots] - ''Plots of all Process Control data''
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub>]


==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==
==== Standard Recipe ====


*[https://docs.google.com/spreadsheets/d/1qXCH1phgvk3-5_5FUqeQaGPERhyS5dn4/edit#gid= STD LS Nitride2 Recipe Parameters]
*[https://docs.google.com/spreadsheets/d/1mobnAIH70a9eFbCkMnza2WfpI2uRUWtLlz0cLK1Ljuo/edit?gid=1554182668#gid=1554182668 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C-new May 2024''
*[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= STD LS Nitride2 Recipe]
*''Old Versions:''
**[//wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]
**[//wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018]


*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Process Control Data</nowiki>]
==== Historical Data ====
**Lists film data, such as dep rate, stress, particle count, refractive index etc.


===== Thin-Film Properties =====
=== Old Data ===


* [https://docs.google.com/spreadsheets/d/17ft9jrHcCFCp2830RsLwQq5lHuupWATXT91SreG8WYY/edit#gid=143856038 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR250C - replaced on May 2024''"
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]
*[https://docs.google.com/spreadsheets/d/16Q6BrPoNiFP0elVoSGwXRfQdHXzAXOgiyqKmEw-4kII/edit#gid=sharing LS Nitride2 Data 2015]
* [https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=1199123007 Old Recipe] - 2019
*[https://docs.google.com/spreadsheets/d/1GZ58eFzD-T8DJ2Nsaj74u6cvawzsOI2DmMit6Z7vqys/edit#gid=sharing LS Nitride2 Data 2016]
*[https://docs.google.com/spreadsheets/d/1gGIWqkCnykPgBc3prhXExT7QcNjWm2HdbTtwugNqm18/edit#gid=sharing LS Nitride2 Data 2017]
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS Nitride2 Data 2018]
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS Nitride2 Data 2019]
*[https://docs.google.com/spreadsheets/d/1muyFsIspqZXB2HXiqG3t39uzeO7A7Srvh4aGdXjwCc4/edit#gid=sharing LS Nitride2 Data 2020]


*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_LDR_250C_Deposition_.28Unaxis_VLR.29 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021
===== Uniformity Data =====


==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness Uniformity 2014]
*[https://docs.google.com/spreadsheets/d/1LpkaOpr7oNoyvxFkineD7i9FspO6LweJMulvZHJM5Zc/edit#gid=sharing LS Nitride2 Thickness Uniformity 2015]
*[https://docs.google.com/spreadsheets/d/1FRzW9BaIPF2D3cxPgjLq8hbvrBHXDNkiW6DiPVKQBRM/edit#gid=sharing LS Nitride2 Thickness Uniformity 2016]
*[https://docs.google.com/spreadsheets/d/1vyrgvdEZFgnQUilpa5Ka2nOfowY8zlmJfbQ77EamNBg/edit#gid=sharing LS Nitride2 Thickness Uniformity 2017]
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2018]
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2019]
*[https://docs.google.com/spreadsheets/d/1TMasE4I--H948aKCWEO1Y3Dw2pCA6-iqQ0km3v_2VFo/edit#gid=sharing LS Nitride2 Thickness Uniformity 2020]


*[https://docs.google.com/spreadsheets/d/1x0mB4ySSUfEAfRehAx7k_k3BJuTMczaRxQgxsTAFfo4/edit?gid=744785272#gid=744785272 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-new May 2024''"
==Amorphous-Si deposition (PECVD #2)==
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.


=== Old Data ===
*[//wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe]
*[https://docs.google.com/spreadsheets/d/13KUlUujEWSLOH54Ibd52YNJPZcAc7ELShI2RAqM6H-Y/edit#gid=117484667 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 HDR250C-replace on May 2024''"
*[//wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Films and Their Stress]
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=1199123007 Old Recipe] - 2019
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_HDR_250C_Deposition_.28Unaxis_VLR.29 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>]


== Cleaning Recipes (PECVD #2) ==
==Gap-Fill SiO<sub>2</sub> [ICP-PECVD]==
''Recipe designed by [https://scholar.google.com/citations?user=kur3-cEAAAAJ&hl=en&oi=ao Warren Jin], please consider our [https://wiki.nanotech.ucsb.edu/wiki/Frequently_Asked_Questions#Publications_acknowledging_the_Nanofab publication policy] if you publish using this recipe.''
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
'''NOTE:''' Please contact tool [[Tony Bosch|supervisor]] before running this recipe - this recipe must often be scheduled to prevent excessive chamber maintenance.
#Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
Able to effectively fill ~1:1 and ~1:2 aspect ratio gaps in Silicon and Glass structures (eg. waveguides/optical gratings) with void-free filling.
#Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
===[//wiki.nanotech.ucsb.edu/w/images/3/34/PECVD2_photo_for_cleaning.png Standard Clean Recipe: "STD CF4/O2 Clean recipe"] ===
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will '''pop up a window for the cleaning time upon running the recipe''' - you do not need to edit the recipe before running it.


The recipe uses a high 400W RF Bias to reduce buildup on corners that causes voids during growth.
=[[ICP-PECVD (Unaxis VLR)]]=
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the [[ICP-PECVD (Unaxis VLR)#Documentation|'''new procedures''']] to ensure low particle counts in the chamber.


*Category = <code>SiO2 GapFill - Std.</code>
The system currently has '''Deuterated Silane (SiD<sub>4</sub>) installed''' - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.
*FLOW: <code>SiO2 GapFill 250C</code>
**Will run the sequence <code>SiO2 GapFill 250C 450W</code>. Do not change this!
*STEP (edit TIME only): <code>SiO2 GapFill 250C</code>
*Deposition rate = 99.968nm/min [9/20/23]


==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==
==== Historical Particulate Data ====
* [https://docs.google.com/spreadsheets/d/1ZzbpDmkOI3IvGuKqyiQIP44sYJ89E3Zs9sLvjxvWMsc/edit#gid=sharing Particulates in Unaxis films @250C-2019]
* [https://docs.google.com/spreadsheets/d/1fMebt-6BfAurcjMv1aDsmm6VgPqokU73_2ReZFqzEEk/edit#gid=sharing Particulates in Unaxis films @250C-2020]


* [https://docs.google.com/spreadsheets/d/1xvXqgFaKT6vH4ZSAfOaqAYnx_qyEqzNZFqTc-OGENzw/edit?gid=1168016715#gid=1168016715 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD]- Standard Recipe</nowiki>] - ''"SiN 250C-v2- New recipe since April 2026"''
==== Standard Recipes ====
**recipe "SiN 250C-v2", sequence "SiN 250C-v2", category "SiN Std."
*[https://docs.google.com/spreadsheets/d/1T_4gaJQ3wHSNptoAtFR1fN0ePwfw3PsQ0DLSjqGeyM4/edit#gid=sharing SiO2 LDR 250C Recipe-2020]
**this film has a low particle count (good for waveguides)
*[https://docs.google.com/spreadsheets/d/1nsdGPpfyZfIesyYG1PIU9uYyuzQWrfpsvVWM6J_H6BI/edit#gid=sharing SiO2 HDR 250C Recipe-2020]
**requires 30sec O2 plasma using PE-II beforehand
*[https://docs.google.com/spreadsheets/d/1UTr93aWx0MjCwVBwRmYjPwo9ASluGQ-OrJhVG_R57aY/edit#gid=sharing SiN 250C Recipe-2020]
**dep.rate=90.86nm/min, refractive index at 632.8nm=2.04372, refractive index at 1550nm=2.00804, stress=-183MPa
*[https://docs.google.com/spreadsheets/d/1MXW7UNpTyk93ucOVQaSun5IX7QaUbSABNHNznb09qw8/edit#gid=sharing SiN LS 250C Recipe-2020]
**Cauchy A=2.004+/-0.0013, B=0.00745+/-0.00072928, C=0.00999+/-0.00011018


* *[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit?gid=1670372499#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
==SiO2 LDR 250C Deposition (Unaxis VLR)==
** Lists film data, such as dep rate, stress, particle count, refractive index etc.
''Low-Deposition Rate SiO<sub>2</sub>''


==== Historical Data ====
=== Old Data ===
*[https://docs.google.com/spreadsheets/d/1Np5uJ1bw81MxHlDD0qs5Jh_hj7nCSznQTsSEELlT414/edit?usp=sharing Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C- replaced on May 2024''"
===== Thin-Film Properties =====
This data is for 780sec long SiO2 LDR (low deposition rate) deposition, and cleaning time is 900sec, following the procedure [[here]].
*[https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=sharing SiO2 LDR 250C 300nm Data-2019]
*[https://docs.google.com/spreadsheets/d/1bU2Gu3x3DNyrq8skMAQZJCsra-IcoDCT0U5D135YPgc/edit#gid=sharing SiO2 LDR 250C 300nm Data-2020]
===== Uniformity Data =====
*[https://docs.google.com/spreadsheets/d/1Xi21OrargcNRthZ2fM_56APB8O599ctDfq5E_6B5Ft0/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2019]
*[https://docs.google.com/spreadsheets/d/1-ytu5R75FAXNfhJZTRuK2eRZyu_L6Hy1BWV2zN6_tRA/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2020]


*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Old Recipe] - 2019
==SiO2 HDR 250C Deposition (Unaxis VLR)==
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_250C_deposition_.28Unaxis_VLR.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021
''High-Deposition Rate SiO<sub>2</sub>''


** Lists film data, such as dep rate, stress, particle count, refractive index etc.
==== Historical Data ====
===== Thin-Film Properties =====
This data is for 180sec long SiO2 HDR ( high deposition rate) deposition, and cleaning time is 900sec, following the procedure [[here]].
*[https://docs.google.com/spreadsheets/d/16s-tUna9xrkKneK1lE-qSPuUHWlDmP6Qu3IngBXP3R8/edit#gid=sharing SiO2 HDR 250C 300nm Data-2019]
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=sharing SiO2 HDR 250C 300nm Data-2020]
===== Uniformity Data =====
*[https://docs.google.com/spreadsheets/d/1Mm_rsTm9xDQ50kZx6X6EZ5dTegUvinq0zFxRtE8B2R4/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2019]
*[https://docs.google.com/spreadsheets/d/1nzVeCKsmgL17zft6axQlixpvsEowJOG7qCnLQm_0XxE/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2020]


==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==
== SiN 250C deposition (Unaxis VLR) ==
==== Historical Data ====
===== Thin-Film Properties =====
This data is for 480sec long SiN deposition, and cleaning time is 1500sec, following the procedure [[here]].
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=sharing SiN 250C 300nm Data-2020]
===== Uniformity Data =====
*[https://docs.google.com/spreadsheets/d/1YAx_Ix84xId8CAhDwZeFT7jLFUwg-BET9aBwg3DxUmQ/edit#gid=sharing Thickness Uniformity SiN 250C 300nm-2020]


*[https://docs.google.com/spreadsheets/d/1xchMuXlPABSKcW-rMau8B-cw_jnJnwI9qpXqDLUQ8sU/edit?gid=1239658204#gid=1239658204 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C-new May 2024''"
== SiN LS 250C Deposition (Unaxis VLR) ==
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
''Low Stress Silicon-Nitride''
**Lists film data, such as dep rate, stress, particle count, refractive index etc.


==== Historical Data ====
=== Old Data ===
* [https://docs.google.com/spreadsheets/d/1JuQlCU-mozIUJx9z9aQdisIJyFhv1r9AWI8EWeOnsPo/edit#gid=82816489 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C - replaced on May 2024''"
''To Be Added''
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Old Recipe] - 2019


==Standard Seasoning Procedure [ICP-PECVD]==
===== Thin-Film Properties =====
You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film].
This data is for 180sec long SiN LS (low stress) deposition, and cleaning time is 1500sec, following the procedure [[here]].
Seasoning recipes:
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=sharing SiN LS 250C 300nm Data-2020]
*[https://docs.google.com/spreadsheets/d/1S01xgtxFEJ4q7GLHfo-96yYKxer8nGlB/edit?gid=1944526099#gid=1944526099 SiO<sub>2</sub> seasoning - Std ]
===== Uniformity Data =====
*[https://docs.google.com/spreadsheets/d/1NDyxH1i9COM2XTryLqYPE9yOekgRslAJUO7o56iTOEQ/edit#gid=sharing Thickness Uniformity SiN LS 250C 300nm-2020]
*[https://docs.google.com/spreadsheets/d/1S3BFJIn9oAq2bxg6PDe9RY_6Fvkc36ki/edit?gid=1218243940#gid=1218243940 SiN seasoning - Std ]


== Cleaning Recipes (Unaxis VLR Dep) ==
==Standard Cleaning Procedure [ICP-PECVD]==
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details.
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details.

* SiNx etches at 20nm/min
* SiO2 etches at 40nm/min
*SiNx etches at 20nm/min
*SiO<sub>2</sub> etches at 40nm/min

===Standard Clean Recipe===

*[https://docs.google.com/spreadsheets/d/1S3DzvJJahNTwGXsn0GDyg2FiourGffiy/edit?gid=2021404224#gid=2021404224 Post Deposition Clean 250C ]

==General Recipe Notes (Unaxis VLR ICP-PECVD)==

*RF1 = Bias
*RF2 = ICP Power
*All recipes start with an Argon pre-clean with 0W bias (gentle), to improve adhesion/nucleation.
*Maximum SiO<sub>2</sub> Dep. thickness allowed: 800nm
**Above this thickness, you must run a chamber clean/season before depositing more onto your product wafer.

Latest revision as of 21:34, 28 September 2026

Back to Vacuum Deposition Recipes.

PECVD 1 (PlasmaTherm 790)

PECVD 1 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #1)

Old Data

SiN deposition (PECVD #1)

Old Data

Low Stress Si3N4 (PECVD#1)

plot of SiN stress and Refractive Index vs. N2 flow.
Example of Si3N4 modified stress via. varying N2 flow.  Refractive index is relatively constant (one outlier), and stress varies continuously from tensile to compressive.  (Demis D. John 2011, Blumenthal Group)

SiOxNy deposition (PECVD #1)

Standard Cleaning Procedure (PECVD #1)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.

The clean is done in two steps:

  1. Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
  2. Load the recipe for plasma cleaning "CF4/O2 Clean" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.
Table of Cleaning Times
Film Dep'd Cleaning Time
SiO2 1 min clean for every 1 min dep
Si3N4 1 min clean for every 7 min dep
SiOxNy Same as SiO2
a-Si Same time as Si3N4

Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.

PECVD 2 (Advanced Vacuum)

PECVD 2 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #2)

  • SiO2 deposition rate at 150C is 35nm/min

SiN deposition (PECVD #2)

Low-Stress SiN deposition (PECVD #2)

Low-Stress Silicon Nitride, Si3N4 (< ±100 MPa)

Low-Stress SiN 3xTime (PECVD #2)

This Low-Stress SiN recipe is more stable over time (months), because each step is 3x longer (so each compressive/tensile layer is thicker), making it less susceptible to RF ignition delays as the grounding strap is etched over time. – 2024-09 Demis & Biljana

Amorphous-Si deposition (PECVD #2)

Standard Cleaning Procedure (PECVD #2)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
  2. Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.

Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


Clean Times (PECVD#2)

Film Deposited Cleaning Time (Dry)
SiO2 1min. clean for every 1min. deposition
Si3N4 1min. clean for every 7min. of deposition
a-Si 2 min clean for every 1min of deposition
a-Si (max 60min dep before breaking it up and cleaning the chamber) Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

Other films:(max 60min long dep. in one single run) If > 29min total dep time

(Season + Dep)

Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

ICP-PECVD (Unaxis VLR)

2020-02: New recipes have been characterized for low particulate count and repeatability.  Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.

Process Control Data (Unaxis ICP-PECVD)

Regularly-run depositions and measurements of film properties over time - executed by NanoFab Interns.

Low Deposition Rate SiO2 [ICP-PECVD]

Old Data

High Deposition Rate SiO2 [ICP-PECVD]

Old Data

Gap-Fill SiO2 [ICP-PECVD]

Recipe designed by Warren Jin, please consider our publication policy if you publish using this recipe.

NOTE: Please contact tool supervisor before running this recipe - this recipe must often be scheduled to prevent excessive chamber maintenance.

Able to effectively fill ~1:1 and ~1:2 aspect ratio gaps in Silicon and Glass structures (eg. waveguides/optical gratings) with void-free filling.

The recipe uses a high 400W RF Bias to reduce buildup on corners that causes voids during growth.

  • Category = SiO2 GapFill - Std.
  • FLOW: SiO2 GapFill 250C
    • Will run the sequence SiO2 GapFill 250C 450W. Do not change this!
  • STEP (edit TIME only): SiO2 GapFill 250C
  • Deposition rate = 99.968nm/min [9/20/23]

Si3N4 [ICP-PECVD]

  • Si3N4 [ICP-PECVD]- Standard Recipe - "SiN 250C-v2- New recipe since April 2026"
    • recipe "SiN 250C-v2", sequence "SiN 250C-v2", category "SiN Std."
    • this film has a low particle count (good for waveguides)
    • requires 30sec O2 plasma using PE-II beforehand
    • dep.rate=90.86nm/min, refractive index at 632.8nm=2.04372, refractive index at 1550nm=2.00804, stress=-183MPa
    • Cauchy A=2.004+/-0.0013, B=0.00745+/-0.00072928, C=0.00999+/-0.00011018

Old Data

    • Lists film data, such as dep rate, stress, particle count, refractive index etc.

Low Stress Si3N4 [ICP-PECVD]

Old Data

Standard Seasoning Procedure [ICP-PECVD]

You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film]. Seasoning recipes:

Standard Cleaning Procedure [ICP-PECVD]

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min

Standard Clean Recipe

General Recipe Notes (Unaxis VLR ICP-PECVD)

  • RF1 = Bias
  • RF2 = ICP Power
  • All recipes start with an Argon pre-clean with 0W bias (gentle), to improve adhesion/nucleation.
  • Maximum SiO2 Dep. thickness allowed: 800nm
    • Above this thickness, you must run a chamber clean/season before depositing more onto your product wafer.