ICP Etching Recipes: Difference between revisions
→ICP Etch 2 (Panasonic E640): added placeholder for Ru etch |
→Ru (Ruthenium) Etch (Panasonic 2): Ru etch PDF |
||
| Line 3: | Line 3: | ||
=[[DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)]]= |
=[[DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)]]= |
||
==High Rate Bosch Etch (DSEIII)== |
==High Rate Bosch Etch (DSEIII)== |
||
*[[media:10-Si Etch Bosch DSEIII.pdf|Bosch Process]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/4/4a/10-Si_Etch_Bosch_DSEIII.pdf Bosch Process] |
|||
==Single-Step Low Etch Rate Smooth Sidewall Process (DSEIII)== |
==Single-Step Low Etch Rate Smooth Sidewall Process (DSEIII)== |
||
*[[media:10-Si Etch Single Step Smooth Sidewall DSEIII.pdf|Single Step Process]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/8/8f/10-Si_Etch_Single_Step_Smooth_Sidewall_DSEIII.pdf Single Step Process] |
|||
=[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|PlasmaTherm/SLR Fluorine Etcher]]= |
=[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|PlasmaTherm/SLR Fluorine Etcher]]= |
||
==Si Etching |
==Si Etching== |
||
*[[media:SLR - SiVertHF.pdf|SiVertHF]] - Si Vertical Etch using C4F8/SF6/CF4 and resist mask |
|||
*[//www.nanotech.ucsb.edu/wiki/images/b/b8/SLR_-_SiVertHF.pdf SiVertHF] - Si Vertical Etch using C4F8/SF6/CF4 and resist mask |
|||
** Etch Rates: Si ≈ 300-350 nm/min; SiO2 ≈ 30-35 nm/min |
|||
**Etch Rates: Si ≈ 300-350 nm/min; SiO2 ≈ 30-35 nm/min |
|||
** 89-90 degree etch angle, ie, vertical. |
|||
**89-90 degree etch angle, ie, vertical. |
|||
==SiO2 Etching== |
==SiO2 Etching== |
||
* Recipes available, to be characterized/added. |
|||
*Recipes available, to be characterized/added. |
|||
=[[ICP Etch 1 (Panasonic E626I)]]= |
=[[ICP Etch 1 (Panasonic E626I)]]= |
||
==SiO<sub>2</sub> Etching (Panasonic 1)== |
==SiO<sub>2</sub> Etching (Panasonic 1)== |
||
*[[media:Panasonic1-SiO-Etch.pdf|SiO<sub>2</sub> Vertical Etch Recipe Parameters - CHF<sub>3</sub> "SiOVert"]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/3/3e/Panasonic1-SiO-Etch.pdf SiO<sub>2</sub> Vertical Etch Recipe Parameters - CHF<sub>3</sub> "SiOVert"] |
|||
**Etch rate ≈ 2300Å/min (users must calibrate) |
**Etch rate ≈ 2300Å/min (users must calibrate) |
||
**Selectivity (SiO2:Photoresist) ≈ greater than 1:1 (users must calibrate) |
**Selectivity (SiO2:Photoresist) ≈ greater than 1:1 (users must calibrate) |
||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/5/5e/Panasonic1-SiO2-Data-Process-Variation-CHF3-revA.pdf SiO<sub>2</sub> CHF<sub>3</sub> Etch Variations] |
||
*[[Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Florine etch of the underneath layer)|Test Data of etching SiO2 with CHF3/CF4/O2]] |
*[[Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Florine etch of the underneath layer)|Test Data of etching SiO2 with CHF3/CF4/O2]] |
||
*[[Test Data of etching SiO2 with CHF3/CF4-ICP1|Test Data of etching SiO2 with CHF3/CF4]] |
*[[Test Data of etching SiO2 with CHF3/CF4-ICP1|Test Data of etching SiO2 with CHF3/CF4]] |
||
==SiN<sub>x</sub> Etching (Panasonic 1)== |
==SiN<sub>x</sub> Etching (Panasonic 1)== |
||
*[[media:Panasonic1-SiN-Etch-Plasma-CF4-O2-ICP-revA.pdf|SiN<sub>x</sub> Etch Rates and Variations - CF<sub>4</sub>-O<sub>2</sub>]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/c/ce/Panasonic1-SiN-Etch-Plasma-CF4-O2-ICP-revA.pdf SiN<sub>x</sub> Etch Rates and Variations - CF<sub>4</sub>-O<sub>2</sub>] |
|||
==Al Etch (Panasonic 1)== |
==Al Etch (Panasonic 1)== |
||
*[[media:Panasonic-1-Al-Etch-RevA.pdf|Al Etch Recipes - Cl<sub>2</sub>BCl<sub>3</sub>]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/3/3b/Panasonic-1-Al-Etch-RevA.pdf Al Etch Recipes - Cl<sub>2</sub>BCl<sub>3</sub>] |
|||
*[[media:32-Reducing AlCl3 Corrosion with CHF3 plasma.pdf|AlCl<sub>3</sub> Erosion Issue and the Solution]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/6/60/32-Reducing_AlCl3_Corrosion_with_CHF3_plasma.pdf AlCl<sub>3</sub> Erosion Issue and the Solution] |
|||
==Cr Etch (Panasonic 1)== |
==Cr Etch (Panasonic 1)== |
||
*[[media:Panasonic-1-Cr-Etch-revA.pdf|Cr Etch Recipes - Cl<sub>2</sub>O<sub>2</sub>]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/8/88/Panasonic-1-Cr-Etch-revA.pdf Cr Etch Recipes - Cl<sub>2</sub>O<sub>2</sub>] |
|||
==Ta Etch (Panasonic 1)== |
==Ta Etch (Panasonic 1)== |
||
*[[media:104 Ta Etch.pdf|Ta Etch Recipe]] - Cl2/BCl3 |
|||
*[//www.nanotech.ucsb.edu/wiki/images/f/f2/104_Ta_Etch.pdf Ta Etch Recipe] - Cl2/BCl3 |
|||
==Ti Etch (Panasonic 1)== |
==Ti Etch (Panasonic 1)== |
||
*[[media:Panasonic-1-Ti-Etch-Deep-RevA.pdf|Ti Deep Etch Recipes - Cl<sub>2</sub>Ar]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/4/47/Panasonic-1-Ti-Etch-Deep-RevA.pdf Ti Deep Etch Recipes - Cl<sub>2</sub>Ar] |
|||
**See [[doi:10.1149/1.2006647|E. Parker, ''et. al.'' Jnl. Electrochem. Soc., 152 (10) C675-C683 2005]]. |
**See [[doi:10.1149/1.2006647|E. Parker, ''et. al.'' Jnl. Electrochem. Soc., 152 (10) C675-C683 2005]]. |
||
==W-TiW Etch (Panasonic 1)== |
==W-TiW Etch (Panasonic 1)== |
||
*[[media:Panasonic1-TiW-W-Etch-Plasma-RIE-RevA.pdf|Ti-TiW Etch Recipes - SF<sub>6</sub>Ar]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/7/76/Panasonic1-TiW-W-Etch-Plasma-RIE-RevA.pdf Ti-TiW Etch Recipes - SF<sub>6</sub>Ar] |
|||
==GaAs-AlGaAs Etch (Panasonic 1)== |
==GaAs-AlGaAs Etch (Panasonic 1)== |
||
*[[media:Panasonic1-GaAs-PhotonicCrystal-RIE-Plasma-Nanoscale-Etch-RevA.pdf|GaAs-Nanoscale Etch Recipe - PR mask - Cl<sub>2</sub>-BCl<sub>3</sub>-Ar]] |
|||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/b/bb/Panasonic1-GaAs-PhotonicCrystal-RIE-Plasma-Nanoscale-Etch-RevA.pdf GaAs-Nanoscale Etch Recipe - PR mask - Cl<sub>2</sub>-BCl<sub>3</sub>-Ar] |
||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/2/26/12-Plasma_Etching_of_AlGaAs-Panasonic_ICP-1-Etcher.pdf AlGaAs Etch Recipes - Cl<sub>2</sub>N<sub>2</sub>] |
||
*[//www.nanotech.ucsb.edu/wiki/images/0/04/Panasonic1-GaAs-Via-Etch-Plasma-RIE-Fast-DRIE-RevA.pdf GaAs DRIE via Etch Recipes - Cl<sub>2</sub>-BCl<sub>3</sub>-Ar PR passivation] |
|||
==GaN Etch (Panasonic 1)== |
==GaN Etch (Panasonic 1)== |
||
*[[media:07-GaN Etch-Panasonic-ICP-1.pdf|GaN Etch Recipes Cl<sub>2</sub>N<sub>2</sub>]] |
|||
*[[media:Panasonic1-GaN-AlGaN-Selective-Etch-Plasma-RIE-ICP-RevA.pdf|GaN Selective Etch over AlGaN Recipes BCl<sub>3</sub>-SF<sub>6</sub>]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/d/d6/07-GaN_Etch-Panasonic-ICP-1.pdf GaN Etch Recipes Cl<sub>2</sub>N<sub>2</sub>] |
|||
== Photoresist and ARC Etching == |
|||
*[//www.nanotech.ucsb.edu/wiki/images/6/60/Panasonic1-GaN-AlGaN-Selective-Etch-Plasma-RIE-ICP-RevA.pdf GaN Selective Etch over AlGaN Recipes BCl<sub>3</sub>-SF<sub>6</sub>] |
|||
==Photoresist and ARC Etching== |
|||
[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_etching_2 Please see the recipes for Panasonic ICP#2] - the same recipes apply. |
[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_etching_2 Please see the recipes for Panasonic ICP#2] - the same recipes apply. |
||
| Line 59: | Line 74: | ||
==SiC Etch (Panasonic 1)== |
==SiC Etch (Panasonic 1)== |
||
*[[media:Panasonic 1-SiC-ICP-RIE-Etch-Plasma-SF6-RevA.pdf|SiC Etch Recipes Ni Mask - SF<sub>6</sub>]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/d/d0/Panasonic_1-SiC-ICP-RIE-Etch-Plasma-SF6-RevA.pdf SiC Etch Recipes Ni Mask - SF<sub>6</sub>] |
|||
==Sapphire Etch (Panasonic 1)== |
==Sapphire Etch (Panasonic 1)== |
||
*[[media:Panasonic1-sapphire-etch-RIE-Plasma-BCl3-ICP-RevA.pdf|Sapphire Etch Recipes Ni and PR Mask - BCl<sub>3</sub>-Cl<sub>2</sub>]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/3/3a/Panasonic1-sapphire-etch-RIE-Plasma-BCl3-ICP-RevA.pdf Sapphire Etch Recipes Ni and PR Mask - BCl<sub>3</sub>-Cl<sub>2</sub>] |
|||
== Old Deleted Recipes == |
|||
==Old Deleted Recipes== |
|||
Since there are a limited number of recipe slots on the tool, we occasionally have to delete old, unused recipes. |
Since there are a limited number of recipe slots on the tool, we occasionally have to delete old, unused recipes. |
||
| Line 73: | Line 90: | ||
==SiO<sub>2</sub> Etching (Panasonic 2)== |
==SiO<sub>2</sub> Etching (Panasonic 2)== |
||
*[[media:Panasonic2-SiOx-Recipe.pdf|SiO<sub>2</sub> Vertical Etch Recipe - CHF<sub>3</sub> "SiOVert"]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/d/d5/Panasonic2-SiOx-Recipe.pdf SiO<sub>2</sub> Vertical Etch Recipe - CHF<sub>3</sub> "SiOVert"] |
|||
**Direct copy of "SiOVert" from ICP#1, [[ICP_Etching_Recipes#SiO2_Etching_.28Panasonic_1.29|see parameters there]]. |
**Direct copy of "SiOVert" from ICP#1, [[ICP_Etching_Recipes#SiO2_Etching_.28Panasonic_1.29|see parameters there]]. |
||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/9/9e/33-Etching_SiO2_with_Vertical_Side-wall.pdf SiO<sub>2</sub> Vertical Etch Recipe#2 - CF<sub>4</sub>/CHF<sub>3</sub>] |
||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/1/1e/Panasonic2-ICP-Plasma-Etch-SiO2-nanoscale-rev1.pdf SiO<sub>2</sub> Nanoscale Etch Recipe - CHF<sub>3</sub>/O<sub>2</sub>] |
||
*[[Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer)|Test Data of etching SiO2 with CHF3/CF4/O2]] |
*[[Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer)|Test Data of etching SiO2 with CHF3/CF4/O2]] |
||
*[[Test Data of etching SiO2 with CHF3/CF4]] |
*[[Test Data of etching SiO2 with CHF3/CF4]] |
||
| Line 82: | Line 100: | ||
==SiN<sub>x</sub> Etching (Panasonic 2)== |
==SiN<sub>x</sub> Etching (Panasonic 2)== |
||
*[[media:Panasonic2-ICP-Plasma-Etch-SiN-nanoscale-rev1.pdf|SiN<sub>x</sub> Nanoscale Etch Recipe - CHF<sub>3</sub>/O<sub>2</sub>]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/0/06/Panasonic2-ICP-Plasma-Etch-SiN-nanoscale-rev1.pdf SiN<sub>x</sub> Nanoscale Etch Recipe - CHF<sub>3</sub>/O<sub>2</sub>] |
|||
==Al Etch (Panasonic 2)== |
==Al Etch (Panasonic 2)== |
||
*[[media:Panasonic-1-Al-Etch-RevA.pdf|Al Etch Recipes - use panasonic 1 parameters, etch rate 50% higher]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/3/3b/Panasonic-1-Al-Etch-RevA.pdf Al Etch Recipes - use panasonic 1 parameters, etch rate 50% higher] |
|||
== Al2O3 Etching (Panasonic 2) == |
|||
[[:Media:Brian Markman - Al2O3 ICP2 Etch Rates 2018.pdf|ALD Al2O3 Etch Rates in BCl3 Chemistry]] (click for plots of etch rate) |
|||
==Al2O3 Etching (Panasonic 2)== |
|||
[//www.nanotech.ucsb.edu/wiki/images/d/d2/Brian_Markman_-_Al2O3_ICP2_Etch_Rates_2018.pdf ALD Al2O3 Etch Rates in BCl3 Chemistry] (click for plots of etch rate) |
|||
''Contributed by Brian Markman, 2018'' |
''Contributed by Brian Markman, 2018'' |
||
* BCl3 = 30sccm |
|||
*BCl3 = 30sccm |
|||
* Pressure = 0.50 Pa |
|||
*Pressure = 0.50 Pa |
|||
* ICP Source RF = 500 |
|||
*ICP Source RF = 500 |
|||
* Bias RF = 50W or 250W (250W can burn PR) |
|||
*Bias RF = 50W or 250W (250W can burn PR) |
|||
* Cooling He Flow/Pressure = 15.0 sccm / 400 Pa |
|||
*Cooling He Flow/Pressure = 15.0 sccm / 400 Pa |
|||
* Etch Rate 50W: 0.66nm/sec |
|||
* |
*Etch Rate 50W: 0.66nm/sec |
||
*Etch Rate 250W: 1.0 nm/sec |
|||
==GaAs Etch (Panasonic 2)== |
==GaAs Etch (Panasonic 2)== |
||
*[[media:16-GaAs etch-ICP-2.pdf|GaAs Etch Recipes - Panasonic 2 - Cl<sub>2</sub>N<sub>2</sub>]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/f/ff/16-GaAs_etch-ICP-2.pdf GaAs Etch Recipes - Panasonic 2 - Cl<sub>2</sub>N<sub>2</sub>] |
|||
== Photoresist and ARC etching == |
|||
==Photoresist and ARC etching== |
|||
Basic recipes for etching photoresist and Bottom Anti-Reflection Coating (BARC) underlayers are as follows: |
Basic recipes for etching photoresist and Bottom Anti-Reflection Coating (BARC) underlayers are as follows: |
||
=== |
===ARC Etching: DUV-42P or AR6=== |
||
* O2 = 40 sccm // 0.5 Pa |
|||
* |
*O2 = 40 sccm // 0.5 Pa |
||
*ICP = 75W // RF = 75W |
|||
* 45 sec for full etching of DUV-42P (same for AR6) |
|||
*45 sec for full etching of DUV-42P (same for AR6) |
|||
=== |
===UV6-0.8 Etching=== |
||
Works very well for photoresist stripping |
Works very well for photoresist stripping |
||
* O2 = 40 sccm // 1.0 Pa |
|||
* ICP = 350W // RF = 100W |
|||
* Etch Rate = 518.5nm / 1min |
|||
* 2m30sec to fully remove with ~200% overetch |
|||
*O2 = 40 sccm // 1.0 Pa |
|||
== Ru (Ruthenium) Etch (Panasonic 2) == |
|||
*ICP = 350W // RF = 100W |
|||
* [[ICP2 Ru Etch|Ru Etch]] - ''Data to Come'' |
|||
*Etch Rate = 518.5nm / 1min |
|||
*2m30sec to fully remove with ~200% overetch |
|||
==Ru (Ruthenium) Etch (Panasonic 2)== |
|||
TALK TO BILL BEFORE PUBLISHING WORK USING THIS ETCH. We are currently writing a paper on this etch. |
|||
*[https://www.nanotech.ucsb.edu/wiki/images/e/e9/194_Ru_Etch_O2%2CCl2.pdf Ru Etch] - ''[[Bill Mitchell]] 2019-09-19'' |
|||
**''BillM is currently writing a publication on this etch - please discuss with [[Bill Mitchell|Bill]] before submitting any publications using this etch.'' |
|||
=[[ICP-Etch (Unaxis VLR)]]= |
=[[ICP-Etch (Unaxis VLR)]]= |
||
==GaAs-AlGaAs Etch (Unaxis VLR) |
==GaAs-AlGaAs Etch (Unaxis VLR)== |
||
*[[media:15-GaAs etch-Unaxis ICP etcher.pdf|GaAs Etch Recipe (Cl<sub>2</sub>N<sub>2</sub> 30C)]] |
|||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/4/4e/15-GaAs_etch-Unaxis_ICP_etcher.pdf GaAs Etch Recipe (Cl<sub>2</sub>N<sub>2</sub> 30C)] |
||
*[//www.nanotech.ucsb.edu/wiki/images/1/1f/14-AlAs-GR-cal_etch-Unaxis_ICP_etcher.pdf AlGaAs Etch Recipe (Cl<sub>2</sub>N<sub>2</sub> 30C)] |
|||
==InP-InGaAs-InAlAs Etch (Unaxis VLR)== |
==InP-InGaAs-InAlAs Etch (Unaxis VLR)== |
||
*[[media:18-InP-based etching-Cl2N2Ar.pdf|InP-based Material Etch Profile (Cl<sub>2</sub>N<sub>2</sub>Ar200C)]] |
|||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/9/90/18-InP-based_etching-Cl2N2Ar.pdf InP-based Material Etch Profile (Cl<sub>2</sub>N<sub>2</sub>Ar200C)] |
||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/a/ad/17-InP%26InGaAs_etch-Cl2H2Ar-Unaxis-VLR.pdf InP-InGaAs Etch Profile (Cl<sub>2</sub>H<sub>2</sub>Ar 200C)] |
||
*[//www.nanotech.ucsb.edu/wiki/images/6/6e/SiO2-Mask_Etch_Recipe_for_Unaxis_Cl2_Etch.pdf Recipe of Etching SiO<sub>2</sub> Mask for Cl<sub>2</sub> Etch (ICP#2)] |
|||
*[[InP Etch Test Result in Details|InP Etch Historical Data (Cl<sub>2</sub>H<sub>2</sub>Ar 200C)]] |
|||
*[[InP Etch Test Result in Details|InP Etch Historical Data (Cl<sub>2</sub>H<sub>2</sub>Ar 200C)]] |
|||
*[[InP Etch Rate and Selectivity (InP/SiO2)|InP Etch Test]] |
*[[InP Etch Rate and Selectivity (InP/SiO2)|InP Etch Test]] |
||
*[ |
*[//www.nanotech.ucsb.edu/wiki/images/a/ac/Lower-Etch-Rate_InP_Etch_using_Unaxis_PM1_tool_at_200_C.pdf Lower etch-rate InP Etch (Cl<sub>2</sub>N<sub>2</sub> 200C)] |
||
==GaN Etch (Unaxis VLR)== |
==GaN Etch (Unaxis VLR)== |
||
*[[media:09-Plasma Etching of GaN-UnaxisPM1.pdf|GaN Etch Recipe (Cl<sub>2</sub>BCl<sub>3</sub>N<sub>2</sub>Ar 85C)]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/d/df/09-Plasma_Etching_of_GaN-UnaxisPM1.pdf GaN Etch Recipe (Cl<sub>2</sub>BCl<sub>3</sub>N<sub>2</sub>Ar 85C)] |
|||
==GaSb Etch (Unaxis VLR)== |
==GaSb Etch (Unaxis VLR)== |
||
| Line 145: | Line 175: | ||
==Bosch and Release Etch (Si Deep RIE)== |
==Bosch and Release Etch (Si Deep RIE)== |
||
*[[media:10-Si Etch Bosch Release DRIE.pdf|Bosch and Release Processes]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/0/02/10-Si_Etch_Bosch_Release_DRIE.pdf Bosch and Release Processes] |
|||
**Ideal for deep (>>1µm), vertical etching of Silicon. Through-wafer etches are possible (requires carrier wafer). |
**Ideal for deep (>>1µm), vertical etching of Silicon. Through-wafer etches are possible (requires carrier wafer). |
||
**Etch rate depends on area of exposed silicon being etched. |
**Etch rate depends on area of exposed silicon being etched. |
||
**Al<sub>2</sub>O<sub>3</sub> mask (ALD or Sputter) has >9000:1 selectivity |
**Al<sub>2</sub>O<sub>3</sub> mask (ALD or Sputter) has >9000:1 selectivity |
||
**SiO<sub>2</sub> (PECVD) mask has ~100:1 selectivity |
**SiO<sub>2</sub> (PECVD) mask has ~100:1 selectivity |
||
**Thermal SiO<sub>2</sub> has ~300:1 selectivity. |
**Thermal SiO<sub>2</sub> has ~300:1 selectivity. |
||
==Single-step Si Etching (not Bosch Process!) (Si Deep RIE)== |
==Single-step Si Etching (not Bosch Process!) (Si Deep RIE)== |
||
*[[media:10-Si_Etch_using_DRIE_(single-step).pdf|Single-step Si Vertical Etch Recipe - SF<sub>6</sub>-C<sub>4</sub>F<sub>8</sub>-Ar]] |
|||
*[//www.nanotech.ucsb.edu/wiki/images/d/d2/10-Si_Etch_using_DRIE_%28single-step%29.pdf Single-step Si Vertical Etch Recipe - SF<sub>6</sub>-C<sub>4</sub>F<sub>8</sub>-Ar] |
|||
Revision as of 19:23, 4 October 2019
Back to Dry Etching Recipes.
DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)
High Rate Bosch Etch (DSEIII)
Single-Step Low Etch Rate Smooth Sidewall Process (DSEIII)
PlasmaTherm/SLR Fluorine Etcher
Si Etching
- SiVertHF - Si Vertical Etch using C4F8/SF6/CF4 and resist mask
- Etch Rates: Si ≈ 300-350 nm/min; SiO2 ≈ 30-35 nm/min
- 89-90 degree etch angle, ie, vertical.
SiO2 Etching
- Recipes available, to be characterized/added.
ICP Etch 1 (Panasonic E626I)
SiO2 Etching (Panasonic 1)
- SiO2 Vertical Etch Recipe Parameters - CHF3 "SiOVert"
- Etch rate ≈ 2300Å/min (users must calibrate)
- Selectivity (SiO2:Photoresist) ≈ greater than 1:1 (users must calibrate)
- SiO2 CHF3 Etch Variations
- Test Data of etching SiO2 with CHF3/CF4/O2
- Test Data of etching SiO2 with CHF3/CF4
SiNx Etching (Panasonic 1)
Al Etch (Panasonic 1)
Cr Etch (Panasonic 1)
Ta Etch (Panasonic 1)
- Ta Etch Recipe - Cl2/BCl3
Ti Etch (Panasonic 1)
W-TiW Etch (Panasonic 1)
GaAs-AlGaAs Etch (Panasonic 1)
- GaAs-Nanoscale Etch Recipe - PR mask - Cl2-BCl3-Ar
- AlGaAs Etch Recipes - Cl2N2
- GaAs DRIE via Etch Recipes - Cl2-BCl3-Ar PR passivation
GaN Etch (Panasonic 1)
Photoresist and ARC Etching
Please see the recipes for Panasonic ICP#2 - the same recipes apply.
Etching of DUV42P at standard spin/bake parameters also completes in 45 seconds.
SiC Etch (Panasonic 1)
Sapphire Etch (Panasonic 1)
Old Deleted Recipes
Since there are a limited number of recipe slots on the tool, we occasionally have to delete old, unused recipes.
If you need to free up a recipe slot, please contact Don and he'll help you find an old recipe to replace. We take photographs of old recipes, and save them in case a group needs to revive the recipe. Contact us if your old recipe went missing.
ICP Etch 2 (Panasonic E640)
Recipes starting points for materials without processes listed can be obtained from Panasonic1 recipe files. The chambers are slightly different, but essentially the same, requiring only small program changes to obtain similar results.
SiO2 Etching (Panasonic 2)
- SiO2 Vertical Etch Recipe - CHF3 "SiOVert"
- Direct copy of "SiOVert" from ICP#1, see parameters there.
- SiO2 Vertical Etch Recipe#2 - CF4/CHF3
- SiO2 Nanoscale Etch Recipe - CHF3/O2
- Test Data of etching SiO2 with CHF3/CF4/O2
- Test Data of etching SiO2 with CHF3/CF4
- Angled SiO2 sidewall recipe
SiNx Etching (Panasonic 2)
Al Etch (Panasonic 2)
Al2O3 Etching (Panasonic 2)
ALD Al2O3 Etch Rates in BCl3 Chemistry (click for plots of etch rate)
Contributed by Brian Markman, 2018
- BCl3 = 30sccm
- Pressure = 0.50 Pa
- ICP Source RF = 500
- Bias RF = 50W or 250W (250W can burn PR)
- Cooling He Flow/Pressure = 15.0 sccm / 400 Pa
- Etch Rate 50W: 0.66nm/sec
- Etch Rate 250W: 1.0 nm/sec
GaAs Etch (Panasonic 2)
Photoresist and ARC etching
Basic recipes for etching photoresist and Bottom Anti-Reflection Coating (BARC) underlayers are as follows:
ARC Etching: DUV-42P or AR6
- O2 = 40 sccm // 0.5 Pa
- ICP = 75W // RF = 75W
- 45 sec for full etching of DUV-42P (same for AR6)
UV6-0.8 Etching
Works very well for photoresist stripping
- O2 = 40 sccm // 1.0 Pa
- ICP = 350W // RF = 100W
- Etch Rate = 518.5nm / 1min
- 2m30sec to fully remove with ~200% overetch
Ru (Ruthenium) Etch (Panasonic 2)
TALK TO BILL BEFORE PUBLISHING WORK USING THIS ETCH. We are currently writing a paper on this etch.
- Ru Etch - Bill Mitchell 2019-09-19
- BillM is currently writing a publication on this etch - please discuss with Bill before submitting any publications using this etch.
ICP-Etch (Unaxis VLR)
GaAs-AlGaAs Etch (Unaxis VLR)
InP-InGaAs-InAlAs Etch (Unaxis VLR)
- InP-based Material Etch Profile (Cl2N2Ar200C)
- InP-InGaAs Etch Profile (Cl2H2Ar 200C)
- Recipe of Etching SiO2 Mask for Cl2 Etch (ICP#2)
- InP Etch Historical Data (Cl2H2Ar 200C)
- InP Etch Test
- Lower etch-rate InP Etch (Cl2N2 200C)
GaN Etch (Unaxis VLR)
GaSb Etch (Unaxis VLR)
Si Deep RIE (PlasmaTherm/Bosch Etch)
This tool does not exist in this configuration any more, so these recipes are for Reference purposes Only!!! The machine was upgraded to be the new Plasma-Therm Fluorine ICP Etcher - the chamber configuration is now different, making these recipes invalid. For Deep Silicon Etching, the Plasma-Therm DSE-iii is often used. Some single-step Silicon etching is still performed on the SLR Fluorine ICP, due to the slower etch rate.
Bosch and Release Etch (Si Deep RIE)
- Bosch and Release Processes
- Ideal for deep (>>1µm), vertical etching of Silicon. Through-wafer etches are possible (requires carrier wafer).
- Etch rate depends on area of exposed silicon being etched.
- Al2O3 mask (ALD or Sputter) has >9000:1 selectivity
- SiO2 (PECVD) mask has ~100:1 selectivity
- Thermal SiO2 has ~300:1 selectivity.