=[[Sputter 3 (AJA ATC 2000-F)]]= |
=[[Sputter 3 (AJA ATC 2000-F)]]= |
||
+ | =Sputter 3 Process Table= |
||
+ | |||
+ | {| class="wikitable sortable" |
||
+ | |- |
||
+ | ! Material !! Etchant !! Rate (nm/min) !! Anisotropy !! Selective to !! Selectivity !! Ref. !! Notes !! Confirmed by !! Extra column |
||
+ | |- |
||
+ | | InP|| HCl:H3PO4(1:3)|| ~1000 || Highly || InGaAs || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example |
||
+ | |- |
||
+ | | InP|| HCl:H3PO4(1:3)|| ~1000 || Highly || InGaAsP || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example |
||
+ | |- |
||
+ | | InP|| H3PO4:HCl(3:1)|| ~1000 || Highly || InGaAs || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example |
||
+ | |- |
||
+ | | InP|| H3PO4:HCl(3:1)|| ~1000 || Highly || InGaAsP || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example |
||
+ | |} |
||
+ | |||
+ | |||
== Ni and Ta Deposition (Sputter 3) == |
== Ni and Ta Deposition (Sputter 3) == |
||
*[[media:24-Ni_and_Ta_Films_using_Sputter-3.pdf|Ni and Ta Deposition Recipe]] |
*[[media:24-Ni_and_Ta_Films_using_Sputter-3.pdf|Ni and Ta Deposition Recipe]] |
Revision as of 11:57, 17 March 2014
Back to Vacuum Deposition Recipes.
Sputter 1 (Custom)
Sputter 2 (SFI Endeavor)
Al Deposition (Sputter 2)
AlNx Deposition (Sputter 2)
Au Deposition (Sputter 2)
TiO2 Deposition (Sputter 2)
Sputter 3 (AJA ATC 2000-F)
Sputter 3 Process Table
Material | Etchant | Rate (nm/min) | Anisotropy | Selective to | Selectivity | Ref. | Notes | Confirmed by | Extra column |
---|---|---|---|---|---|---|---|---|---|
InP | HCl:H3PO4(1:3) | ~1000 | Highly | InGaAs | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | HCl:H3PO4(1:3) | ~1000 | Highly | InGaAsP | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | H3PO4:HCl(3:1) | ~1000 | Highly | InGaAs | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | H3PO4:HCl(3:1) | ~1000 | Highly | InGaAsP | High | Lamponi (p.102) | Example | Jon Doe | Example |
Ni and Ta Deposition (Sputter 3)
Sputter 4 (AJA ATC 2200-V)
W Deposition (Sputter 4)
Sputter 5 (Lesker AXXIS)
Ion Beam Deposition (Veeco NEXUS)
IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc.
All users are required to enter their calibration deps (simple test deps only)
SiO2 deposition (IBD)
- Refractive Index: ≈1.485
- Rate: ≈6.1nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -320MPa (compressive)
Si3N4 deposition (IBD)
- Refractive Index ≈ 2.01
- Rate ≈ 4.5nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -1756MPa (compressive)
Ta2O5 deposition (IBD)
- Refractive Index ≈ 2.10
- Rate ≈7.8nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -140MPa (compressive)
TiO2 deposition (IBD)
- Refractive Index ≈ 2.3-2.4
- Rate ≈ 1.8nm/min
- Recipe: TiO2_dep