Line 44: Line 44:
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]
*[https://docs.google.com/spreadsheets/d/1SkYqOwgjUyMaFBPhuTjMvBTXu0KdQFNmITryF_OVi8o/edit#gid=sharing Nitride2 Data 2015]
*[https://docs.google.com/spreadsheets/d/1SkYqOwgjUyMaFBPhuTjMvBTXu0KdQFNmITryF_OVi8o/edit#gid=sharing Nitride2 Data 2015]
*[https://docs.google.com/spreadsheets/d/1HJszgZyEZR9ZsiJpQM6pdsoQ6pWwI6brXasdmfDRoBQ/edit#gid= sharing Nitride2 Data 2016]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness Uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness Uniformity 2014]
*[https://docs.google.com/spreadsheets/d/14_dYQu3z31fF_oxsUUX8BmDucgv6B07xB3_zqP0HmvM/edit#gid=sharing Nitride2 Thickness Uniformity 2015]
*[https://docs.google.com/spreadsheets/d/14_dYQu3z31fF_oxsUUX8BmDucgv6B07xB3_zqP0HmvM/edit#gid=sharing Nitride2 Thickness Uniformity 2015]

Revision as of 21:25, 8 January 2016

Back to Vacuum Deposition Recipes.

PECVD 1 (PlasmaTherm 790)

SiN deposition (PECVD #1)

SiO2 deposition (PECVD #1)

SiOxNy deposition (PECVD #1)

PECVD 2 (Advanced Vacuum)

SiO2 deposition (PECVD #2)

SiN deposition (PECVD #2)

LS SiN deposition (PECVD #2)

Amorphous-Si deposition (PECVD #2)

ICP-PECVD (Unaxis VLR)

SiN deposition (Unaxis VLR)

SiN (2% SiH4)

50° (pinholes) 100° (pinholes) 250°

SiN (2% SiH4 - No-Ar)

50° (pinholes) 100° (pinholes) 250°

SiN (2% SiH4 - No-Ar - Extra N2)

50° (pinholes) 100° (pinholes) 250°

SiN (100% SiH4 )

50° (pinholes) 100° (pinholes) 250°

SiO2 deposition (Unaxis VLR)

SiO2 (2% SiH4)

50° 100° 250°

SiO2 (2% SiH4 - No Ar)

50° 100° 250°

SiO2 (100% SiH4 HDR)

50° 100° 250°

SiO2 (100% SiH4 LDR)

50° 100° 250°

Amorphous Si (100%SiH4 Ar He)

90° 250°