Vacuum Deposition Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
IBD Al2O3 "R" link
Updated to "new" sputter 5 link
Line 2: Line 2:
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
! width="1675" height="45" colspan="18" | <div style="font-size: 150%;">Vacuum Deposition Recipes</div>
! colspan="18" width="1675" height="45" | <div style="font-size: 150%;">Vacuum Deposition Recipes</div>
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
| <!-- INTENTIONALLY LEFT BLANK --> <br>
| <!-- INTENTIONALLY LEFT BLANK --> <br>
! align="center" bgcolor="#d0e7ff" colspan="4" | '''[[E-Beam Evaporation Recipes|E-Beam Evaporation]]'''
! colspan="4" bgcolor="#d0e7ff" align="center" | '''[[E-Beam Evaporation Recipes|E-Beam Evaporation]]'''
! align="center" bgcolor="#d0e7ff" colspan="6" | '''[[Sputtering Recipes|Sputtering]]'''
! colspan="6" bgcolor="#d0e7ff" align="center" | '''[[Sputtering Recipes|Sputtering]]'''
! align="center" bgcolor="#d0e7ff" colspan="2" | '''[[Thermal Evaporation Recipes|Thermal Evaporation]]'''
! colspan="2" bgcolor="#d0e7ff" align="center" | '''[[Thermal Evaporation Recipes|Thermal Evaporation]]'''
! align="center" bgcolor="#d0e7ff" colspan="3" | '''[[PECVD Recipes|Plasma Enhanced Chemical<br>Vapor Deposition (PECVD)]]'''
! colspan="3" bgcolor="#d0e7ff" align="center" | '''[[PECVD Recipes|Plasma Enhanced Chemical<br>Vapor Deposition (PECVD)]]'''
! width="90" align="center" bgcolor="#d0e7ff" | '''[[Atomic Layer Deposition Recipes|Atomic Layer Deposition]]'''
! width="90" bgcolor="#d0e7ff" align="center" | '''[[Atomic Layer Deposition Recipes|Atomic Layer Deposition]]'''
! width="80" align="center" bgcolor="#d0e7ff" | '''[[Molecular Vapor Deposition Recipes|Molecular Vapor Deposition]]'''
! width="80" bgcolor="#d0e7ff" align="center" | '''[[Molecular Vapor Deposition Recipes|Molecular Vapor Deposition]]'''
|-
|-
! width="20" align="center" bgcolor="#d0e7ff" | '''Material'''
! width="20" bgcolor="#d0e7ff" align="center" | '''Material'''
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]]
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]]
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]]
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]]
Line 21: Line 21:
| width="65" bgcolor="#daf1ff" | [[Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29|Sputter 3<br>(ATC 2000-F)]]
| width="65" bgcolor="#daf1ff" | [[Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29|Sputter 3<br>(ATC 2000-F)]]
| width="65" bgcolor="#daf1ff" | [[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(ATC 2200-V)]]
| width="65" bgcolor="#daf1ff" | [[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(ATC 2200-V)]]
| width="65" bgcolor="#daf1ff" | [[Sputtering Recipes#Sputter_5_.28Lesker_AXXIS.29|Sputter 5 (Lesker AXXIS)]]
| width="65" bgcolor="#daf1ff" | [[Sputter 5 (AJA ATC 2200-V)]]
| width="55" bgcolor="#daf1ff" | [[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]]
| width="55" bgcolor="#daf1ff" | [[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]]
| width="45" bgcolor="#daf1ff" | [[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]]
| width="45" bgcolor="#daf1ff" | [[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]]
Line 31: Line 31:
| width="65" bgcolor="#daf1ff" | [[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]]
| width="65" bgcolor="#daf1ff" | [[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]]
|-
|-
! align="center" bgcolor="#d0e7ff" | Ag
! bgcolor="#d0e7ff" align="center" | Ag
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 50: Line 50:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Al
! bgcolor="#d0e7ff" align="center" | Al
| {{Al/E1}}
| {{Al/E1}}
| <br>
| <br>
Line 69: Line 69:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Al<sub>2</sub>O<sub>3</sub>
! bgcolor="#d0e7ff" align="center" | Al<sub>2</sub>O<sub>3</sub>
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E2}}
| bgcolor="#eeffff" | {{Al/E2}}
Line 88: Line 88:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | AlN
! bgcolor="#d0e7ff" align="center" | AlN
| <br>
| <br>
| <br>
| <br>
Line 107: Line 107:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Au
! bgcolor="#d0e7ff" align="center" | Au
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 126: Line 126:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | B
! bgcolor="#d0e7ff" align="center" | B
| <br>
| <br>
| <br>
| <br>
Line 145: Line 145:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | C
! bgcolor="#d0e7ff" align="center" | C
| align="center" bgcolor="#eeffff" | {{rl|E-Beam Evaporation Recipes|Materials Table (E-Beam #1)}}
| bgcolor="#eeffff" align="center" | {{rl|E-Beam Evaporation Recipes|Materials Table (E-Beam #1)}}
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
| align="center" bgcolor="#eeffff" |
| bgcolor="#eeffff" align="center" |
|-
|-
! align="center" bgcolor="#d0e7ff" | CeO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" | CeO<sub>2</sub>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | {{rl|E-Beam Evaporation Recipes|E-Beam 2 (Custom)|CeO<sub>2</sub> deposition (E-Beam 2)}}
| bgcolor="#eeffff" | {{rl|E-Beam Evaporation Recipes|E-Beam 2 (Custom)|CeO<sub>2</sub> deposition (E-Beam 2)}}
Line 183: Line 183:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Co
! bgcolor="#d0e7ff" align="center" | Co
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 202: Line 202:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Cr
! bgcolor="#d0e7ff" align="center" | Cr
| {{Al/E1}}
| {{Al/E1}}
| <br>
| <br>
Line 221: Line 221:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Cu
! bgcolor="#d0e7ff" align="center" | Cu
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 240: Line 240:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Fe
! bgcolor="#d0e7ff" align="center" | Fe
| {{Al/E1}}
| {{Al/E1}}
| <br>
| <br>
Line 259: Line 259:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Ge
! bgcolor="#d0e7ff" align="center" | Ge
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 278: Line 278:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | GeO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" | GeO<sub>2</sub>
|
|
| {{Al/E2}}
| {{Al/E2}}
Line 297: Line 297:
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | Gd
! bgcolor="#d0e7ff" align="center" | Gd
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 316: Line 316:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Hf
! bgcolor="#d0e7ff" align="center" | Hf
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 335: Line 335:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | HfO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" | HfO<sub>2</sub>
| <br>
| <br>
| <br>
| <br>
Line 354: Line 354:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | In
! bgcolor="#d0e7ff" align="center" | In
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 373: Line 373:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Ir
! bgcolor="#d0e7ff" align="center" | Ir
| {{Al/E1}}
| {{Al/E1}}
| <br>
| <br>
Line 392: Line 392:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | ITO
! bgcolor="#d0e7ff" align="center" | ITO
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | {{rl|E-Beam Evaporation Recipes|E-Beam 2 (Custom)|ITO deposition (E-Beam 2)}}
| bgcolor="#eeffff" | {{rl|E-Beam Evaporation Recipes|E-Beam 2 (Custom)|ITO deposition (E-Beam 2)}}
Line 411: Line 411:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | MgF2
! bgcolor="#d0e7ff" align="center" | MgF2
|
|
|
|
Line 430: Line 430:
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | MgO
! bgcolor="#d0e7ff" align="center" | MgO
|
|
| {{Al/E2}}
| {{Al/E2}}
Line 449: Line 449:
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | Mo
! bgcolor="#d0e7ff" align="center" | Mo
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 468: Line 468:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Nb
! bgcolor="#d0e7ff" align="center" | Nb
| {{Al/E1}}
| {{Al/E1}}
| <br>
| <br>
Line 487: Line 487:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Nd
! bgcolor="#d0e7ff" align="center" | Nd
|
|
| <br>
| <br>
Line 506: Line 506:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Ni
! bgcolor="#d0e7ff" align="center" | Ni
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 525: Line 525:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | NiCr
! bgcolor="#d0e7ff" align="center" | NiCr
| {{Al/E1}}
| {{Al/E1}}
|
|
Line 544: Line 544:
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | NiFe
! bgcolor="#d0e7ff" align="center" | NiFe
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
Line 563: Line 563:
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
|-
|-
! align="center" bgcolor="#d0e7ff" | Pd
! bgcolor="#d0e7ff" align="center" | Pd
| {{Al/E1}}
| {{Al/E1}}
| <br>
| <br>
Line 582: Line 582:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Pt
! bgcolor="#d0e7ff" align="center" | Pt
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 601: Line 601:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Ru
! bgcolor="#d0e7ff" align="center" | Ru
| {{Al/E1}}
| {{Al/E1}}
| <br>
| <br>
Line 620: Line 620:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Si
! bgcolor="#d0e7ff" align="center" | Si
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | {{Al/E2}}
| bgcolor="#eeffff" | {{Al/E2}}
Line 639: Line 639:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | SiN
! bgcolor="#d0e7ff" align="center" | SiN
| <br>
| <br>
| <br>
| <br>
Line 658: Line 658:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | SiO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" | SiO<sub>2</sub>
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E2}}
| bgcolor="#eeffff" | {{Al/E2}}
Line 677: Line 677:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | SiO<sub>x</sub>N<sub>y</sub>
! bgcolor="#d0e7ff" align="center" | SiO<sub>x</sub>N<sub>y</sub>
| <br>
| <br>
| <br>
| <br>
Line 696: Line 696:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Sn
! bgcolor="#d0e7ff" align="center" | Sn
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 715: Line 715:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | SrF<sub>2</sub>
! bgcolor="#d0e7ff" align="center" | SrF<sub>2</sub>
| <br>
| <br>
| {{Al/E2}}
| {{Al/E2}}
Line 734: Line 734:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Ta
! bgcolor="#d0e7ff" align="center" | Ta
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 753: Line 753:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Ta<sub>2</sub>O<sub>5</sub>
! bgcolor="#d0e7ff" align="center" | Ta<sub>2</sub>O<sub>5</sub>
| <br>
| <br>
| <br>
| <br>
Line 772: Line 772:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Ti
! bgcolor="#d0e7ff" align="center" | Ti
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 791: Line 791:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | TiN
! bgcolor="#d0e7ff" align="center" | TiN
| <br>
| <br>
| <br>
| <br>
Line 810: Line 810:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | TiW
! bgcolor="#d0e7ff" align="center" | TiW
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 829: Line 829:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | TiO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" | TiO<sub>2</sub>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | {{Al/E2}}
| bgcolor="#eeffff" | {{Al/E2}}
Line 848: Line 848:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | V
! bgcolor="#d0e7ff" align="center" | V
| <br>
| <br>
| <br>
| <br>
Line 867: Line 867:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | W
! bgcolor="#d0e7ff" align="center" | W
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | {{Al/E1}}
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 886: Line 886:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Zn
! bgcolor="#d0e7ff" align="center" | Zn
| <br>
| <br>
| <br>
| <br>
Line 905: Line 905:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | ZnO
! bgcolor="#d0e7ff" align="center" | ZnO
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 924: Line 924:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | Zr
! bgcolor="#d0e7ff" align="center" | Zr
| {{Al/E1}}
| {{Al/E1}}
| <br>
| <br>
Line 943: Line 943:
| <br>
| <br>
|-
|-
! align="center" bgcolor="#d0e7ff" | ZrO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" | ZrO<sub>2</sub>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
Line 962: Line 962:
| bgcolor="#eeffff" | <br>
| bgcolor="#eeffff" | <br>
|-
|-
! width="20" align="center" bgcolor="#d0e7ff" | '''Material'''
! width="20" bgcolor="#d0e7ff" align="center" | '''Material'''
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]]
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]]
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]]
| width="65" bgcolor="#daf1ff" | [[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]]

Revision as of 21:09, 1 May 2018

  • R = Recipe is available. Clicking this link will take you to the recipe.
  • A = Material is available for use, but no recipes are provided.
Vacuum Deposition Recipes

E-Beam Evaporation Sputtering Thermal Evaporation Plasma Enhanced Chemical
Vapor Deposition (PECVD)
Atomic Layer Deposition Molecular Vapor Deposition
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 1 (Custom) Sputter 2
(SFI Endeavor)
Sputter 3
(ATC 2000-F)
Sputter 4
(ATC 2200-V)
Sputter 5 (AJA ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAL) Molecular Vapor Deposition (Tool)
Ag A
A A

A A








Al A
A A
R1 A R1

A
A A




Al2O3 A A



A R1
R




R1
AlN




R1 A A
A




R1
Au A
A A
R1 A R1

A A




B
















C R1
CeO2
CeO2 deposition (E-Beam 2)














Co A

A

R









Cr A

A

R


A A




Cu A




R1 A








Fe A

A

R









Ge A
A A

A A








GeO2 A
Gd A

A












Hf A















HfO2





A A






R1
In










A




Ir A















ITO
ITO deposition (E-Beam 2)



A A
A






MgF2 A A
MgO A
Mo A




R A








Nb A





R








Nd





A








Ni A
A A

R1


A A




NiCr A A
NiFe A A A
Pd A
A A





A A




Pt A
A A

A R1






R1
Ru A

A












Si
A



R A

A



Amorphous-Si deposition (PECVD#2 R

SiN





R1 A
R

R1 R1 R1

SiO2 A A



R1 A A R

R1 R1 R1 R1
SiOxNy








A

R



Sn










A




SrF2
A














Ta A




R1 A

A







Ta2O5


A




R






Ti A
A A

R1 R1

A







TiN




A
R
A




R1
TiW A




A R1








TiO2
A


R1 A R1
R




R1
V





A A








W A




A R1








Zn









A A




ZnO














R1
Zr A

A

A A








ZrO2














R1
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 1 (Custom) Sputter 2
(SFI Endeavor)
Sputter 3
(ATC 2000-F)
Sputter 4
(ATC 2200-V)
Sputter 5 (Lesker AXXIS) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAl) Molecular Vapor Deposition (Tool)