RIE Etching Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Ningcao (talk | contribs)
→RIE 5 (PlasmaTherm): added Photoressit & ARC etching, copied from DUV Litho recipes page
Line 3: Line 3:
=[[RIE 2 (MRC)]] =
=[[RIE 2 (MRC)]] =
==CdZnTe Etching (RIE 2)==
==CdZnTe Etching (RIE 2)==
*[[media:11-CZT_etching-1.pdf|CdZnTe Etch Recipes - CH<sub>4</sub>-H<sub>2</sub>-Ar]]
*[[media:11-CZT etching-1.pdf|CdZnTe Etch Recipes - CH<sub>4</sub>-H<sub>2</sub>-Ar]]


==ZnS Etching (RIE 2)==
==ZnS Etching (RIE 2)==
*[[media:ZnS_Plasma_Etch-1.pdf|ZnS Etch Recipe - CH<sub>4</sub>-H<sub>2</sub>-Ar]]
*[[media:ZnS Plasma Etch-1.pdf|ZnS Etch Recipe - CH<sub>4</sub>-H<sub>2</sub>-Ar]]


==ITO Etching (RIE 2)==
==ITO Etching (RIE 2)==
Line 22: Line 22:
=[[RIE 5 (PlasmaTherm)]] =
=[[RIE 5 (PlasmaTherm)]] =
==AlGaAs\GaAs Etching (RIE 5)==
==AlGaAs\GaAs Etching (RIE 5)==
*[[media:13-GaAs-AlGaAs_Etching-RIE-5.pdf|GaAs\AlGaAs Etch Recipes - BCl<sub>3</sub>-SiCl<sub>4</sub>]]
*[[media:13-GaAs-AlGaAs Etching-RIE-5.pdf|GaAs\AlGaAs Etch Recipes - BCl<sub>3</sub>-SiCl<sub>4</sub>]]


==GaN Etching (RIE 5)==
==GaN Etching (RIE 5)==
*[[media:08-Plasma_Etching_of_GaN-RIE5.pdf|GaN Etch Recipes - Cl<sub>2</sub>-BCl<sub>3</sub>-Ar]]
*[[media:08-Plasma Etching of GaN-RIE5.pdf|GaN Etch Recipes - Cl<sub>2</sub>-BCl<sub>3</sub>-Ar]]

== Photoresist and ARC ==

=== DUV42P (AR2) etching: ===
* O2 = 20sccm // Pressure = 10mT // RF = 100W // Time = 40 sec
* No need to pump/purge, can etch right away.
* No helium cooling, Run in manual mode.

Revision as of 01:12, 29 September 2018