PECVD Recipes: Difference between revisions
fixed links to pre-2022 historical data |
|||
| Line 6: | Line 6: | ||
==SiO<sub>2</sub> deposition (PECVD #1)== |
==SiO<sub>2</sub> deposition (PECVD #1)== |
||
*[https://docs.google.com/spreadsheets/d/1wloq6HJw5RQIvmeKcBn3xvE_917R6jF_K-btCHjsiIM/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1wloq6HJw5RQIvmeKcBn3xvE_917R6jF_K-btCHjsiIM/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
||
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
||
*[https:// |
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.231.29 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier |
||
==SiN deposition (PECVD #1)== |
==SiN deposition (PECVD #1)== |
||
| Line 17: | Line 16: | ||
*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
||
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=98787450 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=98787450 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
||
*[https:// |
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.231.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier |
||
==Low Stress Si<sub>3</sub>N<sub>4</sub> (PECVD#1)== |
==Low Stress Si<sub>3</sub>N<sub>4</sub> (PECVD#1)== |
||
| Line 23: | Line 22: | ||
*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
||
*[[To Be Added|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]] ''- To Be Added'' |
*[[To Be Added|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]] ''- To Be Added'' |
||
*[https:// |
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#Low-Stress_SiN_-_LS-SiN_.28PECVD.231.29 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - 2021-10 and earlier |
||
==SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1)== |
==SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1)== |
||
| Line 66: | Line 65: | ||
*[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] Standard Recipe</nowiki>] - "''STD SiO2''" |
*[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] Standard Recipe</nowiki>] - "''STD SiO2''" |
||
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=1313651154 SiO<sub>2</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=1313651154 SiO<sub>2</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
||
*[https:// |
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_deposition_.28PECVD_.232.29 SiO<sub>2</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021 |
||
==SiN deposition (PECVD #2)== |
==SiN deposition (PECVD #2)== |
||
| Line 72: | Line 71: | ||
*[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Standard Recipe</nowiki>] - "''Nitride2''" |
*[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Standard Recipe</nowiki>] - "''Nitride2''" |
||
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=773875841 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=773875841 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
||
*[https:// |
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_deposition_.28PECVD_.232.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data</nowiki>] - Before Oct. 2021 |
||
==Low-Stress SiN deposition (PECVD #2)== |
==Low-Stress SiN deposition (PECVD #2)== |
||
| Line 81: | Line 80: | ||
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
||
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=203400760 Plots of Low-Stress Si<sub>3</sub>N<sub>4</sub> Process Control Data] |
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=203400760 Plots of Low-Stress Si<sub>3</sub>N<sub>4</sub> Process Control Data] |
||
*[[ |
*[[Old Deposition Data - 2021-12-15#Low-Stress SiN deposition .28PECVD .232.29|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data - Before Oct. 2021</nowiki>]] |
||
*:''Old Versions of the recipe:'' |
*:''Old Versions of the recipe:'' |
||
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]'' |
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]'' |
||
| Line 129: | Line 128: | ||
*[https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=1199123007 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR 250C''" |
*[https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=1199123007 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiO2 LDR 250C''" |
||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>] |
||
*[https:// |
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_LDR_250C_Deposition_.28Unaxis_VLR.29 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021 |
||
==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]== |
==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]== |
||
| Line 135: | Line 134: | ||
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=1199123007 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiO2 HDR 250C''" |
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=1199123007 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiO2 HDR 250C''" |
||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] Present Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] Present Data</nowiki>] |
||
*[https:// |
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiO2_HDR_250C_Deposition_.28Unaxis_VLR.29 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] Historical Data</nowiki>] |
||
==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
||
| Line 141: | Line 140: | ||
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiN 250C''" |
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiN 250C''" |
||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>] |
||
*[https:// |
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_250C_deposition_.28Unaxis_VLR.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Historical Data</nowiki>] - before Oct. 2021 |
||
==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
||
| Line 147: | Line 146: | ||
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiN Low Stress 250C''" |
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiN Low Stress 250C''" |
||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>] |
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>] |
||
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1024532473 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Historical Data</nowiki>] - before Oct. 2021 |
|||
==Standard Cleaning Procedure [ICP-PECVD]== |
==Standard Cleaning Procedure [ICP-PECVD]== |
||
Revision as of 01:14, 16 November 2022
Back to Vacuum Deposition Recipes.
PECVD 1 (PlasmaTherm 790)
PECVD 1 Process Control Plots - Plots of all process control data
SiO2 deposition (PECVD #1)
- SiO2 [PECVD 1] Current Process Control Data
- SiO2 [PECVD 1] Historical Data - Oct. 2021 and earlier
SiN deposition (PECVD #1)
- Si3N4 [PECVD 1] Standard Recipe
- Si3N4 [PECVD 1] Current Process Control Data
- Si3N4 [PECVD 1] Historical Data - Oct. 2021 and earlier
Low Stress Si3N4 (PECVD#1)
- Low Stress Si3N4 [PECVD 1] Standard Recipe
- Low Stress Si3N4 [PECVD 1] Current Process Control Data - To Be Added
- Low Stress Si3N4 [PECVD 1] Historical Data - 2021-10 and earlier
SiOxNy deposition (PECVD #1)
- SiOxNy Standard Recipe
- SiOxNy Data 2014 - Rate, Index etc.
- SiOxNy1000A Thickness uniformity 2014
Standard Cleaning Procedure (PECVD #1)
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
- Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
- Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
| Film Dep'd | Cleaning Time |
|---|---|
| SiO2 | TBD |
| Si3N4 | TBD |
| SiOxNy | Same as XYZ |
Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
PECVD 2 (Advanced Vacuum)
PECVD 2 Process Control Plots - Plots of all process control data
SiO2 deposition (PECVD #2)
- SiO2 [PECVD 2] Standard Recipe - "STD SiO2"
- SiO2 [PECVD 2] Current Process Control Data
- SiO2 [PECVD 2] Historical Data - Before Oct. 2021
SiN deposition (PECVD #2)
- Si3N4 [PECVD 2] Standard Recipe - "Nitride2"
- Si3N4 [PECVD 2] Current Process Control Data
- Si3N4 [PECVD 2] Historical Data - Before Oct. 2021
Low-Stress SiN deposition (PECVD #2)
Low-Stress Silicon Nitride, Si3N4 (< ±100 MPa)
- Low Stress Si3N4 [PECVD 2] Standard Recipe - "LSNitride2
- Low Stress Si3N4 [PECVD 2] Current Process Control Data
- Plots of Low-Stress Si3N4 Process Control Data
- Low Stress Si3N4 [PECVD 2] Historical Data - Before Oct. 2021
- Old Versions of the recipe:
- LS Nitride2 Standard Recipe 2014-5/9/2018
- STD LSNitride2 5/9/2018
Amorphous-Si deposition (PECVD #2)
Standard Cleaning Procedure (PECVD #2)
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
- (If >29min dep time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again.
- Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.
Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
Clean Times (PECVD#2)
| Film Deposited | Cleaning Time (Dry) |
|---|---|
| SiO2 | 1 min. clean for every 1 min. deposition |
| Si3N4 | 1 min. clean for every 7 min of deposition |
| If > 29min total dep time
(Season + Dep) |
Wet Clean the Upper Lid/Chamber
DI water then Isopropyl Alcohol on chamber wall & portholes |
ICP-PECVD (Unaxis VLR)
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.
ICP-PECVD Process Control Plots - Plots of all Process Control data
Low Deposition Rate SiO2 [ICP-PECVD]
- Low Deposition Rate SiO2 [ICP-PECVD] - Standard Recipe - "SiO2 LDR 250C"
- Low Deposition Rate SiO2 [ICP-PECVD] - Current Process Control Data
- Low Deposition Rate SiO2 [ICP-PECVD] - Historical Data - before Oct. 2021
High Deposition Rate SiO2 [ICP-PECVD]
- High Deposition Rate SiO2 [ICP-PECVD] Standard Recipe - "SiO2 HDR 250C"
- High Deposition Rate SiO2 [ICP-PECVD] Present Data
- High Deposition Rate SiO2 [ICP-PECVD] Historical Data
Si3N4 [ICP-PECVD]
- Si3N4 [ICP-PECVD] Standard Recipe - "SiN 250C"
- Si3N4 [ICP-PECVD] Current Process Control Data
- Si3N4 [ICP-PECVD] Historical Data - before Oct. 2021
Low Stress Si3N4 [ICP-PECVD]
- Low Stress Si3N4 [ICP-PECVD] Standard Recipe - "SiN Low Stress 250C"
- Low Stress Si3N4 [ICP-PECVD] Current Process Control Data
Standard Cleaning Procedure [ICP-PECVD]
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.
- SiNx etches at 20nm/min
- SiO2 etches at 40nm/min
Standard Clean Recipe
To Be Added