Direct-Write Lithography Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
→Greyscale Lithography (MLA150): deleted Flood Expose column
Line 9: Line 9:


'''''Any I-Line PR is usable''''', although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR.
'''''Any I-Line PR is usable''''', although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR.

'''<u>Note:</u>''' On this tool, it is common to have to run a Focus-Exposure Matrix (aka. FEM), via "''Series''" exposure mode, for each new layer structure and/or critical feature size. The layer structure can strongly affect the exposure parameters. See the [[ASML Stepper 3 Standard Operating Procedure#Tips for FEM analysis|FEM Analysis Tips page]] for how to choose the proper exposure parameters.


===Positive Resist (MLA150)===
===Positive Resist (MLA150)===
''We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies, compensate using CD Bias [[MLA150 - Design Guidelines#High-Resolution Writing|as described here]].''
''We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies; compensate for widening/narrowing using CD Bias [[MLA150 - Design Guidelines#High-Resolution Writing|as described here]].''


Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns.
Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns.

Revision as of 00:27, 15 March 2024

Maskless Aligner (Heidelberg MLA150)

Photolithography Recipes for the Heidelberg MLA150. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point.

These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches.

Any I-Line PR is usable, although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR.

Note: On this tool, it is common to have to run a Focus-Exposure Matrix (aka. FEM), via "Series" exposure mode, for each new layer structure and/or critical feature size. The layer structure can strongly affect the exposure parameters. See the FEM Analysis Tips page for how to choose the proper exposure parameters.

Positive Resist (MLA150)

We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies; compensate for widening/narrowing using CD Bias as described here.

Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus Rehydrate* PEB** Developer Developer Time Comments
AZ4110 4 krpm, 30s 95°C, 60s ~ 1.1 µm 405 240 5 none AZ400K:DI 1:4 50s Used HIMT design (good for isolated lines 0.8-1um)
AZ4330 4 krpm, 30s 95°C, 60s ~ 3.3 µm 405 320 6 none AZ400K:DI 1:4 90s Used HIMT design
AZ4620
SPR 220-3.0 2.5 krpm, 30s 115°C, 90s ~ 2.7 µm 405 325 - 4 115°C, 90s AZ300MIF 60s Used HIMT design. 0.6-0.9µm line/space.
SPR 220-7.0 3.5 krpm, 30s 105°C/2min

Cool 1min

~ 7.0µm 375 ~550mJ -20 >1hr 115°C, 90s AZ300MiF 70s Rehydration after exposure is necessary, to prevent bubbles at PEB.
SPR 955-CM0.9 3 krpm, 30s 95°C, 90s ~ 0.9 µm 405 250 - 7 110°C, 90s AZ300MIF 60s Used HIMT design
THMR-3600HP 1.5 krpm, 45s;

250 rpm/s

100°C, 60s 0.430µm 405 180–220 -4 100°C, 60s AZ300MiF 20s ~0.4nm line/space:

lower dose for clear-field, higher dose for dark-field.

*Rehydration: After exposure, leave sample in lab air (ok to cover in tray, with tinfoil). Allows water vapor in air to diffuse into PR to complete chemical reaction.

**PEB: Post-exposure bake: after exposure, before develop

Negative Resist (MLA150)

We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus PEB* Flood* Developer Developer Time Comments
AZ5214 6 krpm, 30s 95°C, 60s ~ 1.0 µm 375 35 - 5 110°C, 60s 60" AZ300MIF 60s Used UCSB design. Good for up to ~1.3um open line space.
AZnLOF2020 4 krpm, 30s 110°C, 60s ~ 2.1µm 375 340 - 3 110°C, 60s none AZ300MIF 90s Used UCSB design. Good for 2um open line space.
SU-8 2075 ~70µm 375 Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end.
*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal, and requires Flood Exposure with the MA6 or MJB aligner afterwards, before developing.

Greyscale Lithography (MLA150)

AZ4620 is the manufacturer-recommended PR for greyscale litho.

Please see the MLA150 - Greyscale Design Guidelines & Limitation

Resist Spin Cond. Bake Thickness Laser Exposure Dose (mJ/cm2) Focus Offset Rehydrate* PEB** Developer Developer Time Reflow*** Comments
AZ4620 ? krpm/30” 95°C, 60” AZ300MIF 60s
  • TBD
SPR 220-7.0 3.5 krpm, 30s 105°C/2min

Cool 1min

~ 7.0µm 375 ~624mJ to clear large mm-area,

520mJ to clear ~5µm lines.

-20 ≥1hr 115°C, 90s AZ300MiF 70s TBD Rehydration after exposure is necessary, to prevent bubbles at PEB.

Stitching leaves ridges in Y-direction with ~5% height of removed PR depth. Can be reduced via reflow.

Author Credit: Patrick Curtis, 2022 & Biljana Stamenic 2023 & Demis D. John 2023

*Rehydration: After exposure, leave sample in lab air (ok to cover in tray, with tinfoil). Allows water vapor in air to diffuse into PR to complete chemical reaction.

**PEB: Post-exposure bake: after exposure, before develop

***Reflow: To smooth out stitching lines. Will change sharp vertical profiles considerably, only good for gradually-sloped profiles.