Sputtering Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
→SiN deposition (IBD): added rate, index, stress
→Ta{{sub|2}}O{{sub|5}} deposition (IBD): added reate, index, stress
Line 24: Line 24:


==Ta{{sub|2}}O{{sub|5}} deposition (IBD)==
==Ta{{sub|2}}O{{sub|5}} deposition (IBD)==
* Refractive Index ≈ 2.10
* Rate ≈7.8nm/min (users must calibrate this prior to critical deps)
* Stress ≈ -140MPa (compressive)

*{{fl|IBD-Ta2O5-Recipe.pdf|Ta{{sub|2}}O{{sub|5}} dep}}
*{{fl|IBD-Ta2O5-Recipe.pdf|Ta{{sub|2}}O{{sub|5}} dep}}



Revision as of 19:44, 13 August 2013

Back to Vacuum Deposition Recipes.

Sputter 1 (Custom)

Sputter 2 (SFI Endeavor)

Sputter 3 (AJA ATC 2000-F)

Sputter 4 (AJA ATC 2200-V)

Sputter 5 (Lesker AXXIS)

Ion Beam Deposition (Veeco NEXUS)

IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc.

SiO2 deposition (IBD)

  • SiO2 dep
  • Refractive Index: ≈1.485
  • Rate: ≈6.1nm/min (users must calibrate this prior to critical deps)
  • Stress ≈ -320MPa (compressive)

SiN deposition (IBD)

  • Refractive Index ≈ 2.01
  • Rate ≈ 4.5nm/min (users must calibrate this prior to critical deps)
  • Stress ≈ -1756MPa (compressive)

Ta2O5 deposition (IBD)

  • Refractive Index ≈ 2.10
  • Rate ≈7.8nm/min (users must calibrate this prior to critical deps)
  • Stress ≈ -140MPa (compressive)

TiO2 deposition (IBD)