Difference between revisions of "OLD - PECVD2 Recipes"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
m (John d moved page PECVD2 Recipes to OLD - PECVD2 Recipes without leaving a redirect: this page is not linked anywhere, looks like 2014 data only)
 
(25 intermediate revisions by one other user not shown)
Line 1: Line 1:
 
=[[PECVD 2 (Advanced Vacuum)]]=
 
=[[PECVD 2 (Advanced Vacuum)]]=
== SiN deposition (PECVD #2) ==
 
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data September 2014]
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]
 
   
  +
==Photos==
*Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
 
  +
*Refractive Index: ≈ 1.957
 
  +
*[[media: Photos Sheet1.pdf|Dirty platen]]
*Stress ≈ 499MPa
 
*HF etch rate:~49nm/min
 
   
 
== SiO<sub>2</sub> deposition (PECVD #2) ==
 
== SiO<sub>2</sub> deposition (PECVD #2) ==
*[[media:Advanced PECVD OXIDE 300C standard recipe OXIDE Standard Recipe.pdf|Oxide Standard Recipe]]
+
*[[media:NewAdvPECVD OXIDE 300C standard recipe.pdf|Oxide Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data August 2014]
+
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]
   
 
== SiN deposition (PECVD #2) ==
*Deposition Rate: ≈ 28.50 nm/min (users must calibrate this prior to critical deps)
 
 
*[[media:NewAdvPECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]
*Refractive Index: ≈ 1.474
 
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]
*Stress ≈ -252MPa
 
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]
*HF etch rate~616nm/min
 
   
 
==LS SiN deposition (PECVD #2) ==
 
==LS SiN deposition (PECVD #2) ==
 
*[[media:NewAdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]
 
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]
*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data August 2014]
 
 
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]
 
*Deposition Rate: ≈ 8.14 nm/min (users must calibrate this prior to critical deps)
 
*Refractive Index: ≈ 1.935
 
*Stress ≈ -7.18MPa
 
*HF etch rate~48nm/min
 
   
 