Vacuum Deposition Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
No edit summary
 
(13 intermediate revisions by 4 users not shown)
Line 3: Line 3:


===Deposition Tools/Materials Table===
===Deposition Tools/Materials Table===
''The Key/Legend for this table's A...R6 values is at the [https://wiki.nanofab.ucsb.edu/wiki/Vacuum_Deposition_Recipes?veaction=edit bottom of the page].''
''The Key/Legend for this table's <code>R1...R6</code> values is at the [[Vacuum Deposition Recipes#Process Ranking Table|<u>bottom of the page</u>]].''
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
Line 34: Line 34:
|-
|-
! bgcolor="#d0e7ff" align="center" |Ag
! bgcolor="#d0e7ff" align="center" |Ag
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E3}}
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 49: Line 49:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!AgBr
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!AgCl
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Al
! bgcolor="#d0e7ff" align="center" |Al
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|{{Al/E1}}
|<br>
|{{Al/E3}}
|{{Al/E4}}
|[[Sputtering Recipes|A]]
|{{rl|Sputtering Recipes|Al Deposition (Sputter 4)}}
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|[[Sputtering Recipes|R1]]
|[[Sputtering Recipes|R3]]
|[[Sputtering Recipes|R1]]
|R1
|R1
|[[Thermal Evaporation Recipes|A]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
|[[Thermal Evaporation Recipes|A]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|<br>
|<br>
|<br>
|<br>
Line 68: Line 102:
|-
|-
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |{{Al/E2}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Al2O3 Deposition (Sputter 4)}}
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]]
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 83: Line 117:
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|R4]]
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|R4]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!As
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!AuPd
|
|
|
|
|
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|
|
|
|
|
|
|-
!AuZn
|
|
|
|
|
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|
|
|
|
|
|
|-
!AuSn
|
|
|
|
|
|
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|
|
|
|
|
|-
!AuGe
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |AlN
! bgcolor="#d0e7ff" align="center" |AlN
Line 89: Line 208:
|<br>
|<br>
|<br>
|<br>
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|<br>
|<br>
|R1
|R1
Line 102: Line 221:
|-
|-
! bgcolor="#d0e7ff" align="center" |Au
! bgcolor="#d0e7ff" align="center" |Au
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E3}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Au|R6]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Ti-Au Deposition (Sputter 4)}}
| bgcolor="#eeffff" |R3
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes|A]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes|A]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 128: Line 247:
|<br>
|<br>
|<br>
|<br>
|
|<br>
|<br>
|<br>
|<br>
Line 133: Line 253:
|<br>
|<br>
|<br>
|<br>
|-
|<br>
!Be
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |C
! bgcolor="#d0e7ff" align="center" |C
| bgcolor="#eeffff" align="center" |{{rl|E-Beam Evaporation Recipes|Materials Table (E-Beam #1)}}
| bgcolor="#eeffff" align="center" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R3]]
| bgcolor="#eeffff" align="center" |
| bgcolor="#eeffff" align="center" |
| bgcolor="#eeffff" align="center" |
| bgcolor="#eeffff" align="center" |
Line 151: Line 287:
| bgcolor="#eeffff" align="center" |
| bgcolor="#eeffff" align="center" |
| bgcolor="#eeffff" align="center" |
| bgcolor="#eeffff" align="center" |
|-
!Cd
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!CdS
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!CdTe
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!CaF2
|
|
|
|
|
|
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |CeO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |CeO<sub>2</sub>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{rl|E-Beam Evaporation Recipes|E-Beam 2 (Custom)|CeO<sub>2</sub> deposition (E-Beam 2)}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 170: Line 374:
|-
|-
! bgcolor="#d0e7ff" align="center" |Co
! bgcolor="#d0e7ff" align="center" |Co
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 187: Line 391:
|-
|-
! bgcolor="#d0e7ff" align="center" |Cr
! bgcolor="#d0e7ff" align="center" |Cr
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
|{{Al/E1}}
|<br>
|<br>
|<br>
|<br>
|[[Process Group - Process Control Data#E-Beam 4: Cr|R6]]
|{{Al/E4}}
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R]
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R3]
|<br>
|<br>
|{{Rl|Sputtering_Recipes|Sputter_5_.28AJA_ATC_2200-V.29|R3}}
|<br>
|<br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
|<br>
|[[Thermal Evaporation Recipes|A]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
|[[Thermal Evaporation Recipes|A]]
|<br>
|<br>
|<br>
|<br>
Line 204: Line 408:
|-
|-
! bgcolor="#d0e7ff" align="center" |Cu
! bgcolor="#d0e7ff" align="center" |Cu
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R2]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 221: Line 425:
|-
|-
! bgcolor="#d0e7ff" align="center" |Fe
! bgcolor="#d0e7ff" align="center" |Fe
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|{{Al/E1}}
|<br>
|<br>
|{{Al/E4}}
|[[Sputtering Recipes|R]]
|<br>
|<br>
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|[[Sputtering Recipes|R3]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|<br>
|<br>
|<br>
|<br>
Line 236: Line 440:
|<br>
|<br>
|<br>
|<br>
|-
!Ga
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!GaAs
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Ge
! bgcolor="#d0e7ff" align="center" |Ge
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E3}}
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 256: Line 494:
! bgcolor="#d0e7ff" align="center" |GeO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |GeO<sub>2</sub>
|
|
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
|{{Al/E2}}
|
|
|
|
Line 272: Line 510:
|-
|-
! bgcolor="#d0e7ff" align="center" |Gd
! bgcolor="#d0e7ff" align="center" |Gd
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 289: Line 527:
|-
|-
! bgcolor="#d0e7ff" align="center" |Hf
! bgcolor="#d0e7ff" align="center" |Hf
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 310: Line 548:
|<br>
|<br>
|<br>
|<br>
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|<br>
|<br>
|<br>
|<br>
Line 321: Line 559:
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R4]]
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R4]]
|<br>
|<br>
|-
!Hg
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |In
! bgcolor="#d0e7ff" align="center" |In
Line 332: Line 587:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes|A]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 338: Line 593:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!InSb
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Ir
! bgcolor="#d0e7ff" align="center" |Ir
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
|{{Al/E1}}
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|
|
|<br>
|<br>
|<br>
|<br>
Line 358: Line 630:
! bgcolor="#d0e7ff" align="center" |ITO
! bgcolor="#d0e7ff" align="center" |ITO
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{rl|E-Beam Evaporation Recipes|E-Beam 2 (Custom)|ITO deposition (E-Beam 2)}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 373: Line 645:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
|-
!KCl
! bgcolor="#d0e7ff" align="center" |MgF2
|
|
|
|
|
|
|
|
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|A]]
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!LiF
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!Mg
|
|
|
|
|
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|
|
|
|
|
|-
! bgcolor="#d0e7ff" align="center" |MgF2
|
|
|
|
|[[Sputtering Recipes|R1]]
|[[Sputtering Recipes|R1]]
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|
|
|
|
Line 392: Line 715:
! bgcolor="#d0e7ff" align="center" |MgO
! bgcolor="#d0e7ff" align="center" |MgO
|
|
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
|{{Al/E2}}
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!Mn
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!MnS
|
|
|
|
|
|
Line 408: Line 765:
|-
|-
! bgcolor="#d0e7ff" align="center" |Mo
! bgcolor="#d0e7ff" align="center" |Mo
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 423: Line 780:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!Na
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!NaCl
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Nb
! bgcolor="#d0e7ff" align="center" |Nb
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|{{Al/E1}}
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Sputtering Recipes|R]]
|[[Sputtering Recipes|R3]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|
|
|<br>
|<br>
|<br>
|<br>
Line 440: Line 831:
|<br>
|<br>
|<br>
|<br>
|-
!NbO5
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Nd
! bgcolor="#d0e7ff" align="center" |Nd
Line 447: Line 855:
|<br>
|<br>
|<br>
|<br>
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|
|
|<br>
|<br>
|<br>
|<br>
Line 459: Line 867:
|-
|-
! bgcolor="#d0e7ff" align="center" |Ni
! bgcolor="#d0e7ff" align="center" |Ni
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E3}}
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}}
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ni|R6]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes|A]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes|A]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 476: Line 884:
|-
|-
! bgcolor="#d0e7ff" align="center" |NiCr
! bgcolor="#d0e7ff" align="center" |NiCr
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|{{Al/E1}}
|
|
|
|
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|{{Al/E4}}
|
|
|
|
|
|
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
|
|
|
|
Line 493: Line 901:
|-
|-
! bgcolor="#d0e7ff" align="center" |NiFe
! bgcolor="#d0e7ff" align="center" |NiFe
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
Line 508: Line 916:
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
|-
!Pb
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!PbS
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Pd
! bgcolor="#d0e7ff" align="center" |Pd
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|{{Al/E1}}
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
|{{Al/E3}}
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|{{Al/E4}}
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Thermal Evaporation Recipes|A]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
|[[Thermal Evaporation Recipes|A]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|<br>
|<br>
|<br>
|<br>
Line 527: Line 969:
|-
|-
! bgcolor="#d0e7ff" align="center" |Pt
! bgcolor="#d0e7ff" align="center" |Pt
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E3}}
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 4 (AJA ATC 2200-V)}}
| bcolor="EEFFFF" |{{rl|Sputtering Recipes|Sputter 5 (AJA ATC 2200-V)}}
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bcolor="EEFFFF" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 544: Line 986:
|-
|-
! bgcolor="#d0e7ff" align="center" |Ru
! bgcolor="#d0e7ff" align="center" |Ru
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|{{Al/E1}}
|<br>
|<br>
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|{{Al/E4}}
|<br>
|<br>
|[[Sputtering Recipes#Ru Deposition .28Sputter 4.29|R]]
|[[Sputtering Recipes#Ru Deposition .28Sputter 4.29|R3]]
|<br>
|<br>
|<br>
|<br>
Line 559: Line 1,001:
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]]
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]]
|<br>
|<br>
|-
!Sb
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!Se
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Si
! bgcolor="#d0e7ff" align="center" |Si
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E2}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R3]
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R3]
Line 582: Line 1,058:
|<br>
|<br>
|<br>
|<br>
|{{rl|Sputtering Recipes|SiN deposition (Sputter 3)}}
|[[Sputtering Recipes|R3]]
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|<br>
|<br>
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]]
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]]
Line 612: Line 1,088:
|-
|-
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |{{Al/E2}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|SiO2 deposition (Sputter 3)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]]
| bgcolor="#eeffff" |[[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R6]]
| bgcolor="#eeffff" |[[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R6]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R6]]
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R6]]
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]]
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]]
Line 627: Line 1,103:
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]]
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!SiO<sub>x</sub>
|
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]]
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
!SiO
|
|
|
|
|
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |SiO<sub>x</sub>N<sub>y</sub>
! bgcolor="#d0e7ff" align="center" |SiO<sub>x</sub>N<sub>y</sub>
Line 655: Line 1,165:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes|A]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 664: Line 1,174:
! bgcolor="#d0e7ff" align="center" |SrF<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |SrF<sub>2</sub>
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
|{{Al/E2}}
|<br>
|<br>
|<br>
|<br>
|<br>
Line 672: Line 1,181:
|<br>
|<br>
|<br>
|<br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|<br>
|<br>
|<br>
|<br>
Line 680: Line 1,190:
|-
|-
! bgcolor="#d0e7ff" align="center" |Ta
! bgcolor="#d0e7ff" align="center" |Ta
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Ta deposition (Sputter 3)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 698: Line 1,208:
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]]
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]]
|<br>
|{{Al/E2}}
|<br>
|<br>
|<br>
|<br>
Line 706: Line 1,216:
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]]
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]]
|<br>
|<br>
|
|<br>
|<br>
|<br>
|<br>
|<br>
Line 714: Line 1,224:
|-
|-
! bgcolor="#d0e7ff" align="center" |Ti
! bgcolor="#d0e7ff" align="center" |Ti
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E3}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="#eeffff" |{{Al/E4}}
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ti|R6]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Ti-Au Deposition (Sputter 4)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 5 (AJA ATC 2200-V)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 736: Line 1,246:
|<br>
|<br>
|<br>
|<br>
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29 R]
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29 R3]
|<br>
|<br>
|R1
|R1
Line 748: Line 1,258:
|-
|-
! bgcolor="#d0e7ff" align="center" |TiW
! bgcolor="#d0e7ff" align="center" |TiW
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|W-TiW Deposition (Sputter 4)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 763: Line 1,273:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!TiO
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |{{Al/E2}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 4 (AJA ATC 2200-V)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]]
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 786: Line 1,313:
|<br>
|<br>
|<br>
|<br>
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|
|<br>
|<br>
|<br>
|<br>
Line 799: Line 1,326:
|-
|-
! bgcolor="#d0e7ff" align="center" |W
! bgcolor="#d0e7ff" align="center" |W
| bgcolor="#eeffff" |{{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]]
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|W deposition (Sputter 4)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 814: Line 1,341:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!WC
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Zn
! bgcolor="#d0e7ff" align="center" |Zn
Line 824: Line 1,368:
|<br>
|<br>
|<br>
|<br>
|[[Thermal Evaporation Recipes|A]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
|[[Thermal Evaporation Recipes|A]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
|<br>
|<br>
|<br>
|<br>
Line 841: Line 1,385:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
Line 848: Line 1,392:
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!ZnS
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! bgcolor="#d0e7ff" align="center" |Zr
! bgcolor="#d0e7ff" align="center" |Zr
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|{{Al/E1}}
|<br>
|<br>
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|{{Al/E4}}
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|[[Sputtering Recipes|A]]
|[[Sputtering Recipes|R1]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|<br>
|<br>
|<br>
|<br>
Line 876: Line 1,437:
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>

Latest revision as of 17:55, 5 March 2025

Process Control Data

See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.

Deposition Tools/Materials Table

The Key/Legend for this table's R1...R6 values is at the bottom of the page.

Vacuum Deposition Recipes

E-Beam Evaporation Sputtering Thermal Evaporation Plasma Enhanced Chemical
Vapor Deposition (PECVD)
Atomic Layer Deposition Molecular Vapor Deposition
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 3
(AJA ATC 2000-F)
Sputter 4
(AJA ATC 2200-V)
Sputter 5 (AJA ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAL) Molecular Vapor Deposition (Tool)
Ag R2
R2 R2 R1 R1

R1 R1




AgBr
AgCl
Al R2
R2 R2 R1 R3 R1 R1 R3 R1




Al2O3 R2

R3 R3 R1 R5




R4
As
AuPd R1
AuZn R1
AuSn R1
AuGe R1
AlN



R1 R1
R1




R4
Au R2
R2 R6 R1 R3

R3 R2




B













Be
C R3
Cd
CdS
CdTe
CaF2 R2
CeO2
R3












Co R2

R2 R3


R1 R1




Cr R1

R6 R3
R3
R3 R2




Cu R1


R3 R2

R2 R1




Fe R2

R2 R3


R1 R1




Ga
GaAs
Ge R2
R2 R2 R1 R1







GeO2 R2
Gd R2

R1










Hf R1


R1











HfO2



R1 R1






R4
Hg
In








R3




InSb
Ir R1

R1








ITO
R3

R1 R1 R1 R1






KCl
LiF
Mg R1 R1
MgF2 R1 R1 R1
MgO R2
Mn
MnS
Mo R2


R3 R1






Na
NaCl
Nb R2



R3






NbO5
Nd



R1






Ni R2
R2 R6 R3
R1
R3 R2




NiCr R2 R2 R3
NiFe R1 R2 R1 R3
Pb
PbS
Pd R2
R2 R2



R3 R1




Pt R2
R2 R2 R3 R3 R3




R4
Ru R2

R2
R3






R4
Sb
Se
Si
R2

R3 R1
R1

R3

SiN



R3 R1
R6

R6 R6 R6

SiN - Low Stress R4 R6 R6
SiO2 R2 R2

R3 R1 R2 R6
R6 R6 R6 R4
SiOx R1
SiO R1 R1
SiOxNy






R3

R4



Sn








R2




SrF2
R2





R1





Ta R1


R3 R1
R1





Ta2O5
R1
R1


R6





Ti R2
R2 R6 R3 R3 R3 R1





TiN




R3
R1




R4
TiW R1


R2 R3








TiO
TiO2
R2

R1 R3
R5



R4
V



R1 R1







W R2


R2 R3







WC
Zn







R3 R2




ZnO










R3
ZnS
Zr R2

R2 R1 R1


R1




ZrO2











R4
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 3
(ATC 2000-F)
Sputter 4
(ATC 2200-V)
Sputter 5 (ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAl) Molecular Vapor Deposition (Tool)

Process Ranking Table

Processes in the table above are ranked by their "Process Maturity Level" as follows:

Process Level Description of Process Level Ranking
A Process Allowed and materials available but never done
R1 Process has been ran at least once
R2 Process has been ran and/or procedure is documented or/and data available
R3 Process has been ran, procedure is documented, and data is available
R4 Process has a documented procedure with regular (≥4x per year) data or lookahead/in-Situ control available
R5 Process has a documented procedure with regular (≥4x per year) data and lookahead/in-Situ control available
R6 Process has a documented procedure, regular ( ≥4x per year) data, and control charts/limits available