Vacuum Deposition Recipes: Difference between revisions
Jump to navigation
Jump to search
No edit summary |
|||
(11 intermediate revisions by 4 users not shown) | |||
Line 3: | Line 3: | ||
===Deposition Tools/Materials Table=== |
===Deposition Tools/Materials Table=== |
||
''The Key/Legend for this table's |
''The Key/Legend for this table's <code>R1...R6</code> values is at the [[Vacuum Deposition Recipes#Process Ranking Table|<u>bottom of the page</u>]].'' |
||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
Line 34: | Line 34: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ag |
! bgcolor="#d0e7ff" align="center" |Ag |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |{{Al/E3}} |
|||
| bgcolor="#eeffff" |{{Al/E4}} |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 49: | Line 49: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!AgBr |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!AgCl |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Al |
! bgcolor="#d0e7ff" align="center" |Al |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|{{Al/E1}} |
|||
|<br> |
|||
|{{Al/E3}} |
|||
|{{Al/E4}} |
|||
|[[Sputtering Recipes|A]] |
|||
|{{rl|Sputtering Recipes|Al Deposition (Sputter 4)}} |
|||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|[[Sputtering Recipes|R1]] |
|||
|[[Sputtering Recipes|R3]] |
|||
|[[Sputtering Recipes|R1]] |
|||
|R1 |
|R1 |
||
|[[Thermal Evaporation Recipes| |
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
|[[Thermal Evaporation Recipes| |
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 68: | Line 102: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Al2O3 Deposition (Sputter 4)}} |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]] |
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 83: | Line 117: | ||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|R4]] |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|R4]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!As |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!AuPd |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!AuZn |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!AuSn |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!AuGe |
|||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |AlN |
! bgcolor="#d0e7ff" align="center" |AlN |
||
Line 89: | Line 208: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|<br> |
|<br> |
||
|R1 |
|R1 |
||
Line 102: | Line 221: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Au |
! bgcolor="#d0e7ff" align="center" |Au |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Au|R6]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |R3 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes| |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes| |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 128: | Line 247: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 133: | Line 253: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|- |
|||
|<br> |
|||
!Be |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |C |
! bgcolor="#d0e7ff" align="center" |C |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R3]] |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
Line 151: | Line 287: | ||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
| bgcolor="#eeffff" align="center" | |
| bgcolor="#eeffff" align="center" | |
||
|- |
|||
!Cd |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!CdS |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!CdTe |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!CaF2 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |CeO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |CeO<sub>2</sub> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 170: | Line 374: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Co |
! bgcolor="#d0e7ff" align="center" |Co |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |{{Al/E4}} |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 187: | Line 391: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Cr |
! bgcolor="#d0e7ff" align="center" |Cr |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
|{{Al/E1}} |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Process Group - Process Control Data#E-Beam 4: Cr|R6]] |
|||
|{{Al/E4}} |
|||
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 |
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R3] |
||
|<br> |
|<br> |
||
|{{Rl|Sputtering_Recipes|Sputter_5_.28AJA_ATC_2200-V.29|R3}} |
|||
|<br> |
|<br> |
||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
|<br> |
|||
|[[Thermal Evaporation Recipes| |
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
||
|[[Thermal Evaporation Recipes|A]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 204: | Line 408: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Cu |
! bgcolor="#d0e7ff" align="center" |Cu |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R2]] |
|||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 221: | Line 425: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Fe |
! bgcolor="#d0e7ff" align="center" |Fe |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|{{Al/E1}} |
|||
|<br> |
|||
|<br> |
|||
|{{Al/E4}} |
|||
|[[Sputtering Recipes|R]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|[[Sputtering Recipes|R3]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 236: | Line 440: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|- |
|||
!Ga |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!GaAs |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ge |
! bgcolor="#d0e7ff" align="center" |Ge |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |{{Al/E3}} |
|||
| bgcolor="#eeffff" |{{Al/E4}} |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 256: | Line 494: | ||
! bgcolor="#d0e7ff" align="center" |GeO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |GeO<sub>2</sub> |
||
| |
| |
||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
|{{Al/E2}} |
|||
| |
| |
||
| |
| |
||
Line 272: | Line 510: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Gd |
! bgcolor="#d0e7ff" align="center" |Gd |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 289: | Line 527: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Hf |
! bgcolor="#d0e7ff" align="center" |Hf |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br>[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 310: | Line 548: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 321: | Line 559: | ||
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R4]] |
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R4]] |
||
|<br> |
|<br> |
||
|- |
|||
!Hg |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |In |
! bgcolor="#d0e7ff" align="center" |In |
||
Line 332: | Line 587: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes| |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 338: | Line 593: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!InSb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ir |
! bgcolor="#d0e7ff" align="center" |Ir |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
|||
|{{Al/E1}} |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
| |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 358: | Line 630: | ||
! bgcolor="#d0e7ff" align="center" |ITO |
! bgcolor="#d0e7ff" align="center" |ITO |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |R1 |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 373: | Line 645: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|- |
||
!KCl |
|||
! bgcolor="#d0e7ff" align="center" |MgF2 |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|[[Sputtering Recipes|A]] |
|||
|[[Sputtering Recipes|A]] |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!LiF |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!Mg |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
! bgcolor="#d0e7ff" align="center" |MgF2 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Sputtering Recipes|R1]] |
|||
|[[Sputtering Recipes|R1]] |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
| |
||
| |
| |
||
Line 392: | Line 715: | ||
! bgcolor="#d0e7ff" align="center" |MgO |
! bgcolor="#d0e7ff" align="center" |MgO |
||
| |
| |
||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
|{{Al/E2}} |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!Mn |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!MnS |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
Line 408: | Line 765: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Mo |
! bgcolor="#d0e7ff" align="center" |Mo |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 423: | Line 780: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!Na |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!NaCl |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Nb |
! bgcolor="#d0e7ff" align="center" |Nb |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|{{Al/E1}} |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R3]] |
||
|<br> |
|||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
| |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 440: | Line 831: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|- |
|||
!NbO5 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Nd |
! bgcolor="#d0e7ff" align="center" |Nd |
||
Line 447: | Line 855: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|<br> |
|||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
| |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 459: | Line 867: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ni |
! bgcolor="#d0e7ff" align="center" |Ni |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |{{Al/E3}} |
|||
| bgcolor="#eeffff" |{{Al/E4}} |
|||
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}} |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ni|R6]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |R1 |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes| |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes| |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 476: | Line 884: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |NiCr |
! bgcolor="#d0e7ff" align="center" |NiCr |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|{{Al/E1}} |
|||
| |
| |
||
| |
| |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|{{Al/E4}} |
|||
| |
|||
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
| |
| |
||
| |
| |
||
Line 493: | Line 901: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |NiFe |
! bgcolor="#d0e7ff" align="center" |NiFe |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
|||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
Line 508: | Line 916: | ||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
|- |
|||
!Pb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!PbS |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Pd |
! bgcolor="#d0e7ff" align="center" |Pd |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|{{Al/E1}} |
|||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
|{{Al/E3}} |
|||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|{{Al/E4}} |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Thermal Evaporation Recipes| |
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
|[[Thermal Evaporation Recipes| |
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 527: | Line 969: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Pt |
! bgcolor="#d0e7ff" align="center" |Pt |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |{{Al/E3}} |
|||
| bgcolor="#eeffff" |{{Al/E4}} |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|A]] |
|||
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 4 (AJA ATC 2200-V)}} |
|||
| bcolor="EEFFFF" |{{rl|Sputtering Recipes|Sputter 5 (AJA ATC 2200-V)}} |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
|||
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
|||
| bcolor="EEFFFF" |[[Sputtering Recipes|R3]] |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 544: | Line 986: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ru |
! bgcolor="#d0e7ff" align="center" |Ru |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|{{Al/E1}} |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|{{Al/E4}} |
|||
|<br> |
|<br> |
||
|[[Sputtering Recipes#Ru Deposition .28Sputter 4.29| |
|[[Sputtering Recipes#Ru Deposition .28Sputter 4.29|R3]] |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 559: | Line 1,001: | ||
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
||
|<br> |
|<br> |
||
|- |
|||
!Sb |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!Se |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Si |
! bgcolor="#d0e7ff" align="center" |Si |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |R1 |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R3] |
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R3] |
||
Line 582: | Line 1,058: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|[[Sputtering Recipes|R3]] |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|<br> |
|<br> |
||
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]] |
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]] |
||
Line 612: | Line 1,088: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]] |
||
| bgcolor="#eeffff" |[[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R6]] |
| bgcolor="#eeffff" |[[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R6]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R6]] |
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R6]] |
||
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]] |
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]] |
||
Line 627: | Line 1,103: | ||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R4]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!SiO<sub>x</sub> |
|||
| |
|||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
!SiO |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |SiO<sub>x</sub>N<sub>y</sub> |
! bgcolor="#d0e7ff" align="center" |SiO<sub>x</sub>N<sub>y</sub> |
||
Line 655: | Line 1,165: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes| |
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 664: | Line 1,174: | ||
! bgcolor="#d0e7ff" align="center" |SrF<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |SrF<sub>2</sub> |
||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
|||
|{{Al/E2}} |
|||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 672: | Line 1,181: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 680: | Line 1,190: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ta |
! bgcolor="#d0e7ff" align="center" |Ta |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |R1 |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 698: | Line 1,208: | ||
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]] |
|||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]] |
|||
|<br> |
|||
|{{Al/E2}} |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 706: | Line 1,216: | ||
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]] |
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]] |
||
|<br> |
|<br> |
||
| |
|||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 714: | Line 1,224: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Ti |
! bgcolor="#d0e7ff" align="center" |Ti |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ti|R6]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |R1 |
| bgcolor="#eeffff" |R1 |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 736: | Line 1,246: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29 |
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29 R3] |
||
|<br> |
|<br> |
||
|R1 |
|R1 |
||
Line 748: | Line 1,258: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |TiW |
! bgcolor="#d0e7ff" align="center" |TiW |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 763: | Line 1,273: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!TiO |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]] |
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R5]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 786: | Line 1,313: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
| |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 799: | Line 1,326: | ||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |W |
! bgcolor="#d0e7ff" align="center" |W |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |[[Sputtering Recipes| |
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]] |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]] |
||
| bgcolor="#eeffff" |<br> |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
|||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 814: | Line 1,341: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!WC |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Zn |
! bgcolor="#d0e7ff" align="center" |Zn |
||
Line 824: | Line 1,368: | ||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Thermal Evaporation Recipes| |
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]] |
||
|[[Thermal Evaporation Recipes| |
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]] |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 841: | Line 1,385: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
Line 848: | Line 1,392: | ||
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]] |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
|- |
|||
!ZnS |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- |
|- |
||
! bgcolor="#d0e7ff" align="center" |Zr |
! bgcolor="#d0e7ff" align="center" |Zr |
||
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]] |
|||
|{{Al/E1}} |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]] |
|||
|{{Al/E4}} |
|||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|[[Sputtering Recipes| |
|[[Sputtering Recipes|R1]] |
||
|<br> |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]] |
|||
|<br> |
|<br> |
||
|<br> |
|<br> |
||
Line 876: | Line 1,437: | ||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" | |
| bgcolor="#eeffff" | |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
||
| bgcolor="#eeffff" |<br> |
| bgcolor="#eeffff" |<br> |
Revision as of 17:55, 5 March 2025
Process Control Data
See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.
Deposition Tools/Materials Table
The Key/Legend for this table's R1...R6
values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
Process Level | Description of Process Level Ranking | ||||||||||
A | Process Allowed and materials available but never done | ||||||||||
R1 | Process has been ran at least once | ||||||||||
R2 | Process has been ran and/or procedure is documented or/and data available | ||||||||||
R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
R4 | Process has a documented procedure with regular (≥4x per year) data or lookahead/in-Situ control available | ||||||||||
R5 | Process has a documented procedure with regular (≥4x per year) data and lookahead/in-Situ control available | ||||||||||
R6 | Process has a documented procedure, regular ( ≥4x per year) data, and control charts/limits available |