Line 3: Line 3:
=[[DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)]]=
=[[DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)]]=


==Process Control Data (DSEiii)==
=== Process Tips ===
'''Si Etching C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/Ar (PlasmaTherm DSEiii)'''


* Use the Santovac oil for mounting small pieces to Silicon carrier wafers, or else your resist will burn! Increases thermal conduction to the cooled carrier wafer. (Full-wafers instead get direct Helium cooling.) Careful that the oil does not get anywhere near the outer clamp that holds the wafer down, or your wafer will get stuck.
*'''STD_Bosch_Si (⭐️Production)''' - 100mm Wafer Si etching with ~50% open area and resist mask
** The oil fully dissolves in Acetone or NMP. You can clean oil off the back by wiping the back of the sample against an ACE-soaked wipe.
**This recipe has 2s Etch A time compared to "'''''Plasma-Therm Standard DSE'''''" (which has 1.5s Etch A) below - this reduced undercut of mask and effect of [https://wiki.nanofab.ucsb.edu/w/images/a/a1/Cal_vs_Legacy_DSE.png aspect ratio on etch rate]. All other recipe parameters are the same.
* See the '''[[ICP Etching Recipes#Process Control Data (DSEiii)|Process Control Data below]]''' - Staff/Intern-run Etches Weekly, tracked over time.

** This tells you whether the chamber and tool are operating properly before you run your etch.
*[https://docs.google.com/spreadsheets/d/1xQcdUH560nT928miZMeP7xxQSwHz_a_EB9s_Kb1LSfg/edit?gid=0#gid=0 Si Etching with C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/Ar - '''Etch Data''']
** You can follow the intern's travelers for details of their etch.
*[https://docs.google.com/spreadsheets/d/1xQcdUH560nT928miZMeP7xxQSwHz_a_EB9s_Kb1LSfg/edit?gid=1804752281#gid=1804752281 Si Etching with C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/Ar - '''Plots'''][[File:DSE plot.png|alt=example of Process Control Charts|none|thumb|[https://docs.google.com/spreadsheets/d/1xQcdUH560nT928miZMeP7xxQSwHz_a_EB9s_Kb1LSfg/edit?gid=1804752281#gid=1804752281 Click for Process Control Charts]]][[File:Copy of 22 013 (1).jpg|alt=Example SEM image|none|thumb|412x412px|Example of 16.32µm Deep Etched Silicon with UV6 Photoresist mask, 2µm Pitch. (Image Credit: Noah Dutra 2024-08)]]
*


==Edge-Bead Removal (DSEiii)==
==Edge-Bead Removal (DSEiii)==
Line 21: Line 19:


==High Rate Bosch Etch (DSEIII)==
==High Rate Bosch Etch (DSEIII)==
*[//wiki.nanotech.ucsb.edu/wiki/images/4/4a/10-Si_Etch_Bosch_DSEIII.pdf Bosch Process Recipe and Characterization] - Standard recipe on the tool.[[File:DSEiii Bosch Ecth SEM Example 01.png|alt=Example SEM image|thumb|188x188px|Example of 100µm Deep Bosch Etched Silicon posts with Al<sub>2</sub>O<sub>3</sub> hard mask. Close inspection shows the horizontal "scalloping" from the cycling nature of the etch. (Image Credit: [[Demis D. John]], 2021-07)]]

**'''STD_Bosch_Si (⭐️Production)''' - Developed 2024-10
*[//wiki.nanotech.ucsb.edu/wiki/images/4/4a/10-Si_Etch_Bosch_DSEIII.pdf Bosch Process Recipe and Characterization] - Standard recipe on the tool.
**Recipe Name: "'''''Plasma-Therm Standard DSE'''''" (''Production'' - copy to your ''Personal'' category)
***Old Recipe Name: "'''''Plasma-Therm Standard DSE'''''" - lower EtchA, less tolerant
**Standard [https://en.wikipedia.org/wiki/Deep_reactive-ion_etching#Bosch_process Bosch Process] for high aspect-ratio, high-selectivity Silicon etching.
**Standard [https://en.wikipedia.org/wiki/Deep_reactive-ion_etching#Bosch_process Bosch Process] for high aspect-ratio, high-selectivity Silicon etching.
**Cycles between polymer deposition "Dep" / Polymer etch "Etch A" / Si etch "Etch B" steps. Step Times gives fine control.
***Cycles between polymer deposition "Dep" / Polymer etch "Etch A" / Si etch "Etch B" steps. Step Times gives fine control.
***To reduce roughening/grassing (black silicon), Increase "''Etch A''" ''t''ime by ~50%. Alternatively, reduce "''Dep''" step time by ~20%.
***To reduce roughening/grassing ("black silicon"), Increase "''Etch A''" ''t''ime by ~50%. Alternatively, reduce "''Dep''" step time by ~20%.
**Patterns with different exposed/etched areas will have different "optimal" parameters.
**Patterns with different exposed/etched areas will have different "optimal" parameters.
**This recipe has 2s Etch A time compared to "'''''Plasma-Therm Standard DSE'''''" (which has 1.5s Etch A) below - this reduced the undercut of mask to ~1% of the etch depth and the effect of [https://wiki.nanofab.ucsb.edu/w/images/a/a1/Cal_vs_Legacy_DSE.png aspect ratio on etch rate]. All other recipe parameters are the same.
**Approx Selectivity to Photoresist: ~80 or better.
**Selectivity to Photoresist ~60.
***Larger open area, lower selectivity and lower etch rate.
**Selectivity to SiO<sub>2</sub> should be higher, not yet measured.
***Thick PR's approx ≥10µm tend to burn, avoid thick PR's. They also make edge-bead removal very difficult.
**Selectivity to Al<sub>2</sub>O<sub>3</sub> is extremely high, >9000. See below TSV process for processing tips with Al<sub>2</sub>O<sub>3</sub> hardmask.
**Selectivity to SiO2 should be higher, not yet measured.
**Selectivity to Al<sub>2</sub>O<sub>3</sub> is extremely high, >9000. See below TSV process for processing notes on this film.
**If you need to pattern all the way to the edge of the wafer, PR won't work because you have to remove the edge-bead of photoresist (see above). Instead use hardmask process (See "Through Silicon Via" etch below).
**If you need to pattern all the way to the edge of the wafer, PR won't work because you have to remove the edge-bead of photoresist (see above). Instead use hardmask process (See "Through Silicon Via" etch below).
**Larger open area → lower selectivity & lower etch rate.
***<1% center to edge variability in etch rate for small open area.
***More variation across wafer for larger open area (eg. plasma dicing)
**Thick PR's approx ≥10µm tend to burn, avoid thick PR's. They also make edge-bead removal very difficult. Instead use an SiO<sub>2</sub> hardmask or the Al<sub>2</sub>O<sub>3</sub>/SiO<sub>2</sub> hardmask below.
{|
|[[File:Plasmatherm DSE - 40um deep Si etch Cal 241007 - 30D 002.jpg|alt=Tilted SEM of 40um deep etch|none|thumb|250x250px|~40µm deep Silicon etch, run as Process Control "EtchCal" (''Process Development and Image: [[Noah Dutra]], 2024-10-07'')]]
|[[File:DSE_16um_Bosch_Etch_-_22_013.jpg|alt=Example SEM image|none|thumb|250x250px|Example of 16.32µm Deep Etched Silicon with 650nm thick UV6 Photoresist mask, 2µm Pitch. (''Image Credit: [[Noah Dutra]] 2024-08'')]]
|}


=== '''Si Etching C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/Ar (PlasmaTherm DSEiii)''' ===
::[[File:DSEiii Bosch Ecth SEM Example 01.png|alt=Example SEM image|none|thumb|465x465px|Example of 100µm Deep Bosch Etched Silicon posts with hard mask. Close inspection shows the horizontal "scalloping" from the cycling nature of the etch. (Image Credit: Demis D. John, 2021-07)]]
[[File:DSE plot.png|alt=example of Process Control Charts|thumb|[https://docs.google.com/spreadsheets/d/1xQcdUH560nT928miZMeP7xxQSwHz_a_EB9s_Kb1LSfg/edit?gid=1804752281#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/1xQcdUH560nT928miZMeP7xxQSwHz_a_EB9s_Kb1LSfg/edit?gid=1804752281#gid=1804752281|232x232px]]
* Recipe: ''STD_Bosch_Si (⭐️Production),'' on 100mm Si Wafer with ~50% open area, photoresist mask, ~40µm deep

*[https://docs.google.com/spreadsheets/d/1xQcdUH560nT928miZMeP7xxQSwHz_a_EB9s_Kb1LSfg/edit?gid=0#gid=0 Si Etching with C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/Ar - '''Etch Data''']
*[https://docs.google.com/spreadsheets/d/1xQcdUH560nT928miZMeP7xxQSwHz_a_EB9s_Kb1LSfg/edit?gid=1804752281#gid=1804752281 Si Etching with C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/Ar - '''Plots''']


===Through Silicon Via (TSV) etch (DSEiii)===
===Through Silicon Via (TSV) etch (DSEiii)===
Line 41: Line 51:


Instead, we recommend the following process with Al<sub>2</sub>O<sub>3</sub> hardmask:
Instead, we recommend the following process with Al<sub>2</sub>O<sub>3</sub> hardmask:
We have a new wafer-mounting process for through-silicon etching, using the UV-Release Dicing tape. Contact [[Demis D. John|staff]] for more info.
<big>'''NOTE''': We have recently found that the wax-mounting process process can leave wax on the wafer clamp, causing the next user's wafer to get stuck and fail transfer! '''<u>DO NOT RUN</u>''' the wax-mounting process without discussing with staff first. ''(Through-wafer process with no wax is still acceptable.)'' -- [[Demis D. John|Demis]] 2024-03-11</big>
-- [[Demis D. John|Demis]] 2026-02-10
'''NOTE''':
'''<u>DO NOT RUN</u>''' the wax-mounting process without discussing with staff first. The wax-mounting process process can leave wax on the wafer clamp, causing the next user's wafer to get stuck and fail transfer!
''(Through-wafer process with no wax is still acceptable.)'' -- [[Demis D. John|Demis]] 2024-03-11

{| class="wikitable"
{| class="wikitable"
! colspan="2" |Process for Through-Wafer Silicon Etching
! colspan="2" |Process for Through-Wafer Silicon Etching
with wax-mounting (small pieces only)
|-
|-
|Process to etch through ~550µm Silicon
|Process to etch through ~550µm Silicon
Line 82: Line 99:
|Also make sure wax thickness is not too thick, of long etches could cause wax to seep out from between the wafers.
|Also make sure wax thickness is not too thick, of long etches could cause wax to seep out from between the wafers.
|-
|-
|DSEiii etch - reduce Dep step to eliminate grassing:
|DSEiii etch - to eliminate grassing:

* Increase EtchA LF-Bias Power and Duration
** EtchA: 300W for 3.5–4sec
** New method as of ~2025
Old method: reduce Dep step:


*Bosch Cycles: Dep: 1.2sec / Etch A: 1.5sec / Etch B: 2.0sec
*Bosch Cycles: Dep: 1.2sec / Etch A: 1.5sec / Etch B: 2.0sec
Line 121: Line 143:
|}
|}


==Single-Step Low Etch Rate Smooth Sidewall Process (DSEIII)==
=== Plasma Dicing (DSEIII) ===
'''''Coming Soon''''': Plasma Dicing process with Dicing Tape as backing film.


This process has been developed by staff, is currently in the final stages of finalizing a public recipe. [[Demis D. John|'''''Contact staff''''']] if you want to use it sooner.

==Silicon: Single-Step, Low Etch Rate, Smooth Sidewall Process (DSEIII)==

*'''SF6-C4F8-CF4 Si Etch v1 (⭐️Production)''' - Developed 2026-01 by [[Noah Dutra]]
**12mT, 20/850W, C4F8/SF6/CF4=68.3/32.5/32.4sccm
**E.R. = 339.4nm/min, Selectivity (to UV6) = 4.9
**Smooth, Vertical, E.R. uniformity is within 5% on wafer
**Tested with 4" wafers that are ~50% open with UV6 PR
*[//wiki.nanotech.ucsb.edu/wiki/images/8/8f/10-Si_Etch_Single_Step_Smooth_Sidewall_DSEIII.pdf Single Step Silicon Etch Recipe and Characterization]
*[//wiki.nanotech.ucsb.edu/wiki/images/8/8f/10-Si_Etch_Single_Step_Smooth_Sidewall_DSEIII.pdf Single Step Silicon Etch Recipe and Characterization]
**Older, alternate Si "shallow/smooth" etch recipe.
**Recipe Name: "'''''Nano Trench Etch'''''" (''Production'' - copy to your ''Personal'' category)
**Recipe Name: "'''''Nano Trench Etch'''''" (''Production'' - copy to your ''Personal'' category)
**Used instead of Bosch Process, to avoid scalloping on the sidewall.
**Used instead of Bosch Process, to avoid scalloping on the sidewall.
**Lower selectivity, lower etch rate, smoother sidewalls.
**Lower selectivity, lower etch rate, smoother sidewalls.


== SiO2 Etch (DSEiii) ==
=[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|PlasmaTherm/SLR Fluorine Etcher]]=
These recipes were developed to serve as secondary pathways to the calibrated FICP SiO2 and Si etch calibrations [[Process Group - Process Control Data#PlasmaTherm SLR Fluorine Etcher - Process Control|here]]. [https://wiki.nanofab.ucsb.edu/w/images/b/b3/FICP-DSE_Analogous_Recipes.pdf Click here for SEMs comparing both cals].
*'''CF4-C4F8 SiO2 Etch v1 (⭐️Production)''' - Developed 2026-01 by [[Noah Dutra]]
**3mT, 70/800W, C4F8/CF4=7.5/32.5sccm
**E.R. = 270nm/min, Selectivity (to SPR955) = 1.3
**Vertical/Smooth
**Tested by mounting 1cmx1cm piece with oil on 4" Si


==F-ICP Backup Recipes (DSEiii)==
===Recipe Tips===
These recipes were developed to serve as backup processes for the calibrated [[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|'''Fluorine-ICP''']] SiO2 and Si etches [[Process Group - Process Control Data#PlasmaTherm SLR Fluorine Etcher - Process Control|here]].


[https://wiki.nanofab.ucsb.edu/w/images/b/b3/FICP-DSE_Analogous_Recipes.pdf Click here for SEMs comparing FICP to DSE etch processes].
*RF1: Bias Power (with DCV readback)
*RF2: ICP Power
*For trouble igniting ICP plasma, add 15 to 75 W of bias power during ignition step. Typical ignition pressures 5 to 10 mT.


*'''[[ICP Etching Recipes#Single-Step Low Etch Rate Smooth Sidewall Process (DSEIII)|Si Etch v1 (⭐️Production)]]'''
==Process Control Data (Fluorine ICP Etcher)==
*'''[[ICP Etching Recipes#SiO2 Etch (DSEiii)|SiO2 Etch v1 (⭐️Production)]]'''


===SiO<sub>2</sub> Etching with CHF3/CF4 (Fluorine ICP Etcher)===
=[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|PlasmaTherm/SLR Fluorine Etcher]]=


=== Process Tips ===
*[https://docs.google.com/spreadsheets/d/15hYkCqL3UNNayt4sXrvVi4mBj-OSdnF7PE29mQW9AEY/edit?usp=sharing SiO<sub>2</sub> Etching with CHF3/CF4 - '''Etch Data''']
*[https://docs.google.com/spreadsheets/d/15hYkCqL3UNNayt4sXrvVi4mBj-OSdnF7PE29mQW9AEY/edit#gid=1804752281 SiO<sub>2</sub> Etching with CHF3/CF4 - '''Plots'''][[File:FL-ICP Process Control Data Example.jpg|alt=example of Process Control Charts|none|thumb|242x242px|[https://docs.google.com/spreadsheets/d/15hYkCqL3UNNayt4sXrvVi4mBj-OSdnF7PE29mQW9AEY/edit#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/15hYkCqL3UNNayt4sXrvVi4mBj-OSdnF7PE29mQW9AEY/edit#gid=1804752281]]


* Use the Santovac oil for mounting small pieces to Silicon carrier wafers, or else your resist will burn! Increases thermal conduction to the cooled carrier wafer. (Full-wafers instead get direct Helium cooling.) Careful that the oil does not get anywhere near the outer clamp that holds the wafer down, or your wafer will get stuck.
==Si Etching (Fluorine ICP Etcher)==
** The oil fully dissolves in Acetone or NMP. You can clean oil off the back by wiping the back of the sample against an ACE-soaked wipe.
'''Si Etching C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/CF<sub>4</sub> (Fluorine ICP Etcher)'''
* '''[[Process Group - Process Control Data#PlasmaTherm SLR Fluorine Etcher - Process Control|Process Control Data for this tool]]''' - [[Process Group Internships|Intern-run Etches Weekly]], tracked over time.
** SiO2 and Silicon etche performance is regularly tracked.
** This tells you whether the chamber and tool are operating properly before you run your etch.
** You can follow the intern's travelers for details of their etch.


===Recipe Tips===
*'''SiVertHFv2 (⭐️Production)''' - Full Wafer Si etching with ~50% open area and resist mask
**This recipe has 2x gas flow compared to "'''''SiVertHF'''''" below - this reduced the loading effect (dependence on % etched area).


*RF1: Bias Power (with DCV readback)
*[https://docs.google.com/spreadsheets/d/15iRs-JhfgkMto5rZVtG0hJjcLMiHy039_ahv2nus0UQ/edit?gid=0#gid=0 Si Etching with C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/CF<sub>4</sub> - '''Etch Data''']
*RF2: ICP Power
*[https://docs.google.com/spreadsheets/d/15iRs-JhfgkMto5rZVtG0hJjcLMiHy039_ahv2nus0UQ/edit?gid=1804752281#gid=1804752281 Si Etching with C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/CF<sub>4</sub> - '''Plots'''][[File:FICP-Si.png|alt=example of Process Control Charts|none|thumb|242x242px|[https://docs.google.com/spreadsheets/d/15iRs-JhfgkMto5rZVtG0hJjcLMiHy039_ahv2nus0UQ/edit?gid=1804752281#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/15iRs-JhfgkMto5rZVtG0hJjcLMiHy039_ahv2nus0UQ/edit?gid=1804752281#gid=1804752281]][[File:PRStrip 019 (1).jpg|alt=Example SEM image|none|thumb|412x412px|Example of 1.65µm Deep Etched Silicon, 2µm Pitch. (Image Credit: Noah Dutra 2024-09)]]
*For trouble igniting ICP plasma, add 15 to 75 W of bias power during ignition step. Typical ignition pressures 5 to 10 mT.
*[//wiki.nanotech.ucsb.edu/wiki/images/b/b8/SLR_-_SiVertHF.pdf SiVertHF] - Si Vertical Etch using C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/CF<sub>4</sub> and resist mask

==Si Etch Recipes (Fluorine ICP Etcher)==
[[File:PRStrip 019 (1).jpg|alt=Example SEM image|thumb|180x180px|Example of 1.65µm Deep Etched Silicon, 2µm Pitch. (Image Credit: Noah Dutra 2024-09)]]
*'''"SiVertHFv2" (⭐️Production)'''
**20mTorr, RF=18W, ICP=950W, C4F8/SF6/CF4=120/48/54sccm
***This recipe has 2x gas flow compared to "'''''SiVertHF'''''" below - this reduced the loading effect (dependence on % etched area).
**Selectivity Silicon:Photoresist ≈ 5
**Etch Rates: Si ≈ 300-350 nm/min; SiO<sub>2</sub> ≈ 30-35 nm/min
**Etch Rates: Si ≈ 300-350 nm/min; SiO<sub>2</sub> ≈ 30-35 nm/min
**89-90 degree etch angle, ie, vertical.
**89-90 degree etch angle, ie, vertical.
**High selectivity to Al2O3 masks.
**High selectivity to Al2O3 masks.
***For high aspect ratio Si etching, try [[Atomic Layer Deposition (Oxford FlexAL)|ALD]] [[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|Al<sub>2</sub>O<sub>3</sub>]] (~20-30nm) + [[Atomic Layer Deposition Recipes#SiO2 deposition .28ALD CHAMBER 3.29|SiO<sub>2</sub>]] (2nm, for PR adhesion) hardmasks followed by [https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 Pan2 Al<sub>2</sub>O<sub>3</sub> etch] (will go straight through the thin SiO<sub>2</sub> without additional etch time). Works well for allowing thin PR's (eg. [[Stepper 3 (ASML)|DUV]] or [[E-Beam Lithography System (JEOL JBX-6300FS)|EBL]] PR's) to enable deep etches.
***For high aspect ratio Si etching, try [[Atomic Layer Deposition (Oxford FlexAL)|ALD]] [[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|Al<sub>2</sub>O<sub>3</sub>]] (~20-30nm) + [[Atomic Layer Deposition Recipes#SiO2 deposition .28ALD CHAMBER 3.29|SiO<sub>2</sub>]] (2nm, for PR adhesion) hardmasks followed by [https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 Pan2 Al<sub>2</sub>O<sub>3</sub> etch] (will go straight through the thin SiO<sub>2</sub> without additional etch time). Works well for allowing thin PR's (eg. [[Stepper 3 (ASML)|DUV]] or [[E-Beam Lithography System (JEOL JBX-6300FS)|EBL]] PR's) to enable deep etches.
**[[ICP Etching Recipes#Process Control: Si Etching C4F8/SF6/CF4 (Fluorine ICP Etcher)|Process Control Data below]] - Staff/Intern-run Etches Weekly, tracked over time (with no BARC layer).
*Old Recipe: [//wiki.nanotech.ucsb.edu/wiki/images/b/b8/SLR_-_SiVertHF.pdf SiVertHF] - Si Vertical Etch using C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/CF<sub>4</sub> and resist mask


===Process Notes/Observations===
===Process Notes/Observations===


*Due to high selectivity against SiO2, it may be necessary to run a ~10sec 50W SiO<sub>2</sub> etch (below) to remove native oxide on Si. This can be performed ''in situ'' before the Si etch.
*Due to high selectivity against SiO2, it may be necessary to run a ~10sec 50W SiO<sub>2</sub> etch (below) to remove native oxide on Si. This can be performed ''in situ'' before the Si etch. It's possible this is actually an effect of photoresist open-area - we have conflicting results.
**If you see very low etch rates, try the above SiO2 etch, or try a short [[ICP Etching Recipes#PR/BARC Etch (Fluorine ICP Etcher)|PR/BARC etch]].
*We have observed that full-wafers with small open area in ''photoresist masks'' might require a recalibration of the C4F8/SF6 ratio in order to prevent very low etch rates.
*We have observed that full-wafers with small open area in ''photoresist masks'' might require a recalibration of the C4F8/SF6 ratio in order to prevent very low etch rates.


==SiO2 Etching (Fluorine ICP Etcher)==
=== Process Control: Si Etching C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/CF<sub>4</sub> (Fluorine ICP Etcher) ===
[[File:FICP-Si.png|alt=example of Process Control Charts|thumb|242x242px|[https://docs.google.com/spreadsheets/d/15iRs-JhfgkMto5rZVtG0hJjcLMiHy039_ahv2nus0UQ/edit?gid=1804752281#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/15iRs-JhfgkMto5rZVtG0hJjcLMiHy039_ahv2nus0UQ/edit?gid=1804752281#gid=1804752281]]''Full Wafer Si etching with ~50% open area and resist mask, run weekly by [[Process Group Interns|NanoFab Interns]].''


*[https://docs.google.com/spreadsheets/d/15iRs-JhfgkMto5rZVtG0hJjcLMiHy039_ahv2nus0UQ/edit?gid=0#gid=0 Si Etching with C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/CF<sub>4</sub> - '''Etch Data''']
*[//wiki.nanotech.ucsb.edu/w/images/f/f6/SiO2_Etch%2C_Ru_HardMask_-_Fluorine_ICP_Etch_Process_-_Ning_Cao_2019-06.pdf SiO2 Etching using Ruthenium Hardmask] - Full Process Traveler
*[https://docs.google.com/spreadsheets/d/15iRs-JhfgkMto5rZVtG0hJjcLMiHy039_ahv2nus0UQ/edit?gid=1804752281#gid=1804752281 Si Etching with C<sub>4</sub>F<sub>8</sub>/SF<sub>6</sub>/CF<sub>4</sub> - '''Plots''']
**''Ning Cao & Bill Mitchell, 2019-06''

**''High-selectivity and deep etching using sputtered Ru hardmask and I-Line litho.''
==SiO2 Etch Recipes (Fluorine ICP Etcher)==
**''Etch also works well with PR masking''
[[File:FL-ICP_50W_SiO2_etch_with_Ru_Hard_Mask.png|alt=SEM of FL-ICP 50W SiO2 etch with Ru Hard Mask|thumb|266x266px|50W SiO2 Etch w/ Ru Hardmask]]
**''Chemistry: CHF3/CF4''
[[File:FL-ICP_200W_SiO2_Etch_with_Ru_Hardmask_-_Ning_Cao.png|alt=SEM of FL-ICP 200W SiO2 Etch with Ru Hardmask - Ning Cao|thumb|266x266px|200W SiO2 Etch w/ Ru Hardmask (Ning Cao)]]
**''Variations in SiO<sub>2</sub> etch Bias Power: 50 / 200 / 400W bias.''
*'''"SiO<sub>2</sub> Etch-50W" (⭐️Production)'''
**Ru etch selectivity to PR: 0.18 (less than 1): 150nm Ru / 800nm PR
**3.8mT, RF=50W, ICP=900W, CHF3/CF4=10/30sccm
**50W Bias: ('''recommended''')
**SiO<sub>2</sub> etch rate: ~250nm/min
***Selectivity to photoresist: 1.10–1.20
***SiO<sub>2</sub> selectivity to Ru: 36
**Selectivity SiO<sub>2</sub>:Photoresist ≈ 1.10–1.20
***SiO<sub>2</sub> etch rate: 263nm/min
**Selectivity SiO<sub>2</sub>:Ru ≈ 36
**[[ICP Etching Recipes#SiO2 Etching with CHF3/CF4 (Fluorine ICP Etcher)|Process Control Data Above]] - Staff/Intern-run Etches Weekly, tracked over time.
**200W Bias:

***SiO<sub>2</sub> selectivity to Ru: 38
=== [//wiki.nanotech.ucsb.edu/w/images/f/f6/SiO2_Etch%2C_Ru_HardMask_-_Fluorine_ICP_Etch_Process_-_Ning_Cao_2019-06.pdf SiO<sub>2</sub> Etching using Ruthenium Hardmask] ===
***SiO<sub>2</sub> etch rate: 471nm/min

**This etch is detailed in the following article: [[Template:Publications#Highly Selective and Vertical Etch of Silicon Dioxide using Ruthenium Films as an Etch Mask|W.J. Mitchell ''et al.'', JVST-A, May 2021]]
* Click above for [http://wiki.nanotech.ucsb.edu/w/images/f/f6/SiO2_Etch%2C_Ru_HardMask_-_Fluorine_ICP_Etch_Process_-_Ning_Cao_2019-06.pdf Full Process Traveler]
** Process written for Sputtered Ru & I-Line GCA Stepper litho
** Can be transferred to ALD Ru or DUV/EBL Litho.

*''Ning Cao & Bill Mitchell, 2019-06''
*''High-selectivity and deep etching using sputtered Ru hardmask and I-Line litho.''
*''Etch also works well with PR masking''
*''Chemistry: CHF3/CF4''
*''Variations in SiO<sub>2</sub> etch Bias Power: 50 / 200 / 400W bias.''
*Ru etch selectivity to PR: 0.18 (less than 1): 150nm Ru / 800nm PR
*50W Bias: ('''recommended''')
**Selectivity to photoresist: 1.10–1.20
**SiO<sub>2</sub> selectivity to Ru: 36
**SiO<sub>2</sub> etch rate: 263nm/min
**''Smoothest vertical etch for SiO2.''
*200W Bias: (higher etch rate)
**SiO<sub>2</sub> selectivity to Ru: 38
**SiO<sub>2</sub> etch rate: 471nm/min
*This etch is detailed in the following article: [[Template:Publications#Highly Selective and Vertical Etch of Silicon Dioxide using Ruthenium Films as an Etch Mask|W.J. Mitchell ''et al.'', JVST-A, May 2021]]
*Updates: Many users have found that SiO2-masking the Ru hardmask results in vastly improved photoresist selectivity, making litho+etch of small features much better.
**Layer stack looks like: SiO2 (or other dielectric target layer to etch) / Ru hardmask / SiO2 hardmask (thin) / Photoresist.
**Typically strip the masks+PR with all dry etching. That means the entire etch process (all etches and strips) can be run ''in situ'' on the Panasonic ICP in a rapid single-tool etch process.
===Process Control: SiO<sub>2</sub> Etching with CHF3/CF4 (Fluorine ICP Etcher)===
[[File:FL-ICP Process Control Data Example.jpg|alt=example of Process Control Charts|thumb|242x242px|[https://docs.google.com/spreadsheets/d/15hYkCqL3UNNayt4sXrvVi4mBj-OSdnF7PE29mQW9AEY/edit#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/15hYkCqL3UNNayt4sXrvVi4mBj-OSdnF7PE29mQW9AEY/edit#gid=1804752281]]''Full Wafer Si etching with ~50% open area and resist mask, run weekly by [[Process Group Interns|NanoFab Interns]].''
*[https://docs.google.com/spreadsheets/d/15hYkCqL3UNNayt4sXrvVi4mBj-OSdnF7PE29mQW9AEY/edit?usp=sharing SiO<sub>2</sub> Etching with CHF3/CF4 - '''Etch Data''']
*[https://docs.google.com/spreadsheets/d/15hYkCqL3UNNayt4sXrvVi4mBj-OSdnF7PE29mQW9AEY/edit#gid=1804752281 SiO<sub>2</sub> Etching with CHF3/CF4 - '''Plots''']


==Si<sub>3</sub>N<sub>4</sub> Etching (Fluorine ICP Etcher)==
==Si<sub>3</sub>N<sub>4</sub> Etching (Fluorine ICP Etcher)==
Line 194: Line 272:


===PR/BARC Etch (Fluorine ICP Etcher)===
===PR/BARC Etch (Fluorine ICP Etcher)===
[[File:SEM Image.png|thumb|<u>New PR Strip recipe</u>: Wafer had UV6 or UVN30 as mask. 5min Si etch followed by '''PostBARC Etch/PR Strip (STD)_V2''' with 2min over etch (Credit: [[Gopikrishnan G M|Gopi Meena]])]]

[[File:SEM Image of wafer after PR strip.png|thumb|294x294px|<u>Old PR strip recipe</u>: Wafer had UV6 or UVN30 as mask. 5min Si etch followed by '''PostBARC Etch/PR Strip (STD)''' with 2min over etch (Credit: [[Gopikrishnan G M|Gopi Meena]])]]
*Etching [[Stepper Recipes#DUV-42P|DUV42P-6]] Bottom Anti-Reflection Coating
*Etching [[Stepper Recipes#DUV-42P|DUV42P-6]] Bottom Anti-Reflection Coating
**~60nm thick (2500krpm)
**~60nm thick (2500krpm)
**O2=20sccm / 10mT / RF1(bias)=100W / RF2(icp)=0W
**O2=20sccm / 10mT / RF1(bias)=100W / RF2(icp)=0W
**1min
**45sec-1min


===Photoresist Strip/Polymer Removal (Fluorine ICP Etcher)===
=== Photoresist Strip/Polymer Removal (Fluorine ICP Etcher) ===
'''Old''' PR strip recipe: '''PostBARC Etch/PR Strip (STD)'''
*O2=100sccm / 5mT / RF1(bias)=10W / RF2(icp)=825W
*75W Bias can be helpful for difficult to remove polymers, eg. 2min
*Use laser monitor to check for complete removal, overetch to remove Fluorocarbon polymers.
*Not able to completely remove PR (both negative & positive) after prolonged over etching (over etching of +2min)
*Leaves behind residue on the sides


'''New''' PR strip recipe: '''PostBARC Etch/PR Strip (STD)_V2'''
**O2=100sccm / 5mT / RF1(bias)=10W / RF2(icp)=825W
*O2=100sccm / 5mT / RF1(bias)=100W / RF2(icp)=825W
**75W Bias can be helpful for difficult to remove polymers, eg. 2min
*RF bias increased by 10x to 100W
**Use laser monitor to check for complete removal, overetch to remove Fluorocarbon polymers.
*Able to completely remove PR (both negative & positive) after over etching (over etching of +2min)
*Clean surface with no residue
==W Etching (Fluorine ICP Etcher)==
[[File:W FICP Etch 2.jpg|thumb|223x223px|W Etch. Image Credit: Fatt Foong]]
<code>Developed by Fatt Foong. Please see [[Frequently Asked Questions#Publications acknowledging the Nanofab|publication policy]].</code>


*ICP = 950/15W
==Cleaning Procedures (Fluorine ICP Etcher)==
*Pressure = 10mT
''To Be Added''
*C4F8/SF6/CF4 = 25/40/27sccm
**Etch Rate = 128nm/min


=[[ICP Etch 1 (Panasonic E646V)]]=


==Process Control Data (Panasonic 1)==


==Cleaning Procedures (Fluorine ICP Etcher)==
===SiO<sub>2</sub> Etch with CHF<sub>3</sub>/CF<sub>4</sub> - Process Control Data (Panasonic 1)===


* [https://wiki.nanotech.ucsb.edu/w/images/6/69/Cleaning_Rules_for_Fluorine_ICP_Etch_tool.pdf '''Cleaning Rules'''] - for various etches. All cleans are O2 plasma.
*[https://docs.google.com/spreadsheets/d/1gBqCYXSl7IqpNL-yI11cuURlfZpTWwXUVM9hY_gGpT8/edit?usp=sharing SiO<sub>2</sub> Etch with CHF<sub>3</sub>/CF<sub>4</sub> - '''Etch Data''']

*[https://docs.google.com/spreadsheets/d/1gBqCYXSl7IqpNL-yI11cuURlfZpTWwXUVM9hY_gGpT8/edit#gid=1804752281 SiO<sub>2</sub> Etch with CHF<sub>3</sub>/CF<sub>4</sub> - '''Plots'''][[File:ICP1 Process Control Data Example.jpg|alt=example chart of ICP1 SiO2 Process Control Chart|none|thumb|250x250px|[https://docs.google.com/spreadsheets/d/1gBqCYXSl7IqpNL-yI11cuURlfZpTWwXUVM9hY_gGpT8/edit#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/1gBqCYXSl7IqpNL-yI11cuURlfZpTWwXUVM9hY_gGpT8/edit#gid=1804752281]]
=[[ICP Etch 1 (Panasonic E646V)]]=
'''Panasonic ICP#1 is currently down -''' Use Panasonic ICP#2 instead. Most processes directly transfer with only small change in etch rate. Data kept here for historical purposes only.


==SiO<sub>2</sub> Etching (Panasonic 1)==
==SiO<sub>2</sub> Etching (Panasonic 1)==
Line 229: Line 321:
''Use these to determine how each etch parameter affects the process.''
''Use these to determine how each etch parameter affects the process.''


*[//wiki.nanotech.ucsb.edu/wiki/images/5/5e/Panasonic1-SiO2-Data-Process-Variation-CHF3-revA.pdf SiO<sub>2</sub> CHF<sub>3</sub> Etch Variations] - CHF3 with varying Bias and Pressure, Slanted SiO2 etching
*[//wiki.nanotech.ucsb.edu/wiki/images/5/5e/Panasonic1-SiO2-Data-Process-Variation-CHF3-revA.pdf SiO<sub>2</sub> CHF<sub>3</sub> Etch Variations] - CHF3 with varying Bias and Pressure & Slanted SiO2 etching


==SiN<sub>x</sub> Etching (Panasonic 1)==
==SiN<sub>x</sub> Etching (Panasonic 1)==
Line 289: Line 381:
If you need to free up a recipe slot, please contact the [[ICP Etch 1 (Panasonic E626I)|tool's Supervisor]] and they'll help you find an old recipe to replace. We take photographs of old recipes, and save them in case a group needs to revive the recipe. Contact us if your old recipe went missing.
If you need to free up a recipe slot, please contact the [[ICP Etch 1 (Panasonic E626I)|tool's Supervisor]] and they'll help you find an old recipe to replace. We take photographs of old recipes, and save them in case a group needs to revive the recipe. Contact us if your old recipe went missing.


=[[ICP Etch 2 (Panasonic E626I)]]=
==Process Control Data (Panasonic 1)==
Recipes starting points for materials without processes listed can be obtained from Panasonic1 recipe files. The chambers are slightly different, but essentially the same, requiring only small program changes to obtain similar results.


==Process Control Data (Panasonic 2)==
===SiO<sub>2</sub> Etch with CHF<sub>3</sub>/CF<sub>4</sub> - Process Control Data (Panasonic 1)===


===SiO<sub>2</sub> Etch with CHF<sub>3</sub>/CF<sub>4</sub> - Process Control Data (Panasonic 2)===
*[https://docs.google.com/spreadsheets/d/1gBqCYXSl7IqpNL-yI11cuURlfZpTWwXUVM9hY_gGpT8/edit?usp=sharing SiO<sub>2</sub> Etch with CHF<sub>3</sub>/CF<sub>4</sub> - '''Etch Data''']
*[https://docs.google.com/spreadsheets/d/1gBqCYXSl7IqpNL-yI11cuURlfZpTWwXUVM9hY_gGpT8/edit#gid=1804752281 SiO<sub>2</sub> Etch with CHF<sub>3</sub>/CF<sub>4</sub> - '''Plots'''][[File:ICP1 Process Control Data Example.jpg|alt=example chart of ICP1 SiO2 Process Control Chart|none|thumb|250x250px|[https://docs.google.com/spreadsheets/d/1gBqCYXSl7IqpNL-yI11cuURlfZpTWwXUVM9hY_gGpT8/edit#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/1gBqCYXSl7IqpNL-yI11cuURlfZpTWwXUVM9hY_gGpT8/edit#gid=1804752281]]


=[[ICP Etch 2 (Panasonic E626I)]]=
*[https://docs.google.com/spreadsheets/d/1m0l_UK2lDxlgww4f6nfXe4aQedNeDZsLs46jQ5wR4zw/edit?usp=sharing SiO2 Etch with CHF3/CF4 - '''Etch Data''']
Recipes starting points for materials without processes listed can be obtained from Panasonic1 recipe files. The chambers are slightly different, but essentially the same, requiring only small program changes to obtain similar results.
*[https://docs.google.com/spreadsheets/d/1m0l_UK2lDxlgww4f6nfXe4aQedNeDZsLs46jQ5wR4zw/edit#gid=1804752281 SiO2 Etch with CHF3/CF4 - '''Plots'''][[File:ICP2 Process Control Data Example.jpg|alt=example ICP2 process control chart|none|thumb|250x250px|[https://docs.google.com/spreadsheets/d/1m0l_UK2lDxlgww4f6nfXe4aQedNeDZsLs46jQ5wR4zw/edit#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/1m0l_UK2lDxlgww4f6nfXe4aQedNeDZsLs46jQ5wR4zw/edit#gid=1804752281]]


=== Process Tips ===
==SiO<sub>2</sub> Etching (Panasonic 2)==


* Use the Santovac oil for mounting small pieces to Silicon carrier wafers, or else your resist will burn! Increases thermal conduction to the cooled carrier wafer. (Full-wafers instead get direct Helium cooling.) Careful that the oil does not get on the ''back'' of the carrier wafer or you will get Helium cooling errors.
===Recipes===
** The oil fully dissolves in Acetone or NMP. You can clean oil off the back by wiping the back of the sample against an ACE-soaked wipe.

* See the '''Process Control sections below''' - [[Process Group Interns|NanoFab Interns]] run Etches Weekly, tracked over time.
*[//wiki.nanotech.ucsb.edu/wiki/images/d/d5/Panasonic2-SiOx-Recipe.pdf SiO<sub>2</sub> Vertical Etch Recipe - CHF<sub>3</sub> "SiOVert"]
** This tells you whether the chamber and tool are operating properly before you run your etch.
**Direct copy of "SiOVert" from ICP#1, [[ICP_Etching_Recipes#SiO2_Etching_.28Panasonic_1.29|see parameters there]].
** You can follow the intern's travelers for details of their etch, and see their SEM's.
*[//wiki.nanotech.ucsb.edu/wiki/images/9/9e/33-Etching_SiO2_with_Vertical_Side-wall.pdf SiO<sub>2</sub> Vertical Etch Recipe#2 - CF<sub>4</sub>/CHF<sub>3</sub>]
*[//wiki.nanotech.ucsb.edu/wiki/images/1/1e/Panasonic2-ICP-Plasma-Etch-SiO2-nanoscale-rev1.pdf SiO<sub>2</sub> Nanoscale Etch Recipe - CHF<sub>3</sub>/O<sub>2</sub>]

===Recipe Variations===
''Use these to determine how etch parameters affect the process.''

*[https://wiki.nanotech.ucsb.edu/wiki/images/1/1e/05-SiO2_Nano-structure_Etch.pdf Angled SiO2 sidewall recipes]

==SiN<sub>x</sub> Etching (Panasonic 2)==

*[//wiki.nanotech.ucsb.edu/wiki/images/0/06/Panasonic2-ICP-Plasma-Etch-SiN-nanoscale-rev1.pdf SiN<sub>x</sub> Nanoscale Etch Recipe - CHF<sub>3</sub>/O<sub>2</sub>]


==Al Etch (Panasonic 2)==
==Al Etch (Panasonic 2)==
Line 333: Line 415:
*Etch Rate 50W: 39.6nm/min (0.66nm/sec)
*Etch Rate 50W: 39.6nm/min (0.66nm/sec)
*Etch Rate 250W: 60.0nm/min (1.0 nm/sec)
*Etch Rate 250W: 60.0nm/min (1.0 nm/sec)

== Cr Etching (Panasonic 2) ==

* Cl<sub>2</sub>=48, O<sub>2</sub>=12sccm, 1.33Pa, ICP=600W, RF=50W
** Recipe #154 (please revert when done)
* Handles larger area etching with less loading effect
* Etch Rate: 24–33 nm/min
* Use PR mask. selectivity not measured but ~500nm PR works easily for etching ~85nm Cr.
* Strip PR in O2 plasma (in situ optional): [[ICP Etching Recipes#Photoresist Etch/Strip (Panasonic 2)|Photoresist Etch/Strip (Panasonic 2)]]
* [[Laser Etch Monitoring|Laser Monitor]] recommended


==GaAs Etch (Panasonic 2)==
==GaAs Etch (Panasonic 2)==


*GaAs Etch Cal - ''Noah Dutra & Fatt Foong, 2025-02-12''
*[//wiki.nanotech.ucsb.edu/wiki/images/f/ff/16-GaAs_etch-ICP-2.pdf GaAs Etch Recipes - Panasonic 2 - Cl<sub>2</sub>N<sub>2</sub>]
**Etch Rates ~1um/min, Selectivity to SiO2 ~ 27:1, Sidewalls ~ 90°
**Etch Rate/Selectivity [https://wiki.nanofab.ucsb.edu/w/images/7/76/GaAs_pressure_experiment.png highly sensitive to pressure] (image credit: Terry Guerrero)
**Cal Sample: ~1cm sample etched mounted with oil onto 150mm Si carrier
**Recipe: 0.5Pa, 100/900W, N2/Cl2=10/20sccm
*[//wiki.nanotech.ucsb.edu/wiki/images/f/ff/16-GaAs_etch-ICP-2.pdf Non-Calibration GaAs Etch Recipes - Panasonic 2 - Cl<sub>2</sub>N<sub>2</sub>]

===Process Control: GaAs Etch with N<sub>2</sub>/Cl<sub>2</sub> (Panasonic 2)===
[[File:GaAs Etch ICP2 SPC.png|alt=example ICP2 process control chart|thumb|249x249px|[https://docs.google.com/spreadsheets/d/16gHOO3PQn_LinrXGPeSTSBf5dnw3leSLh1gq0PLr43w/edit?gid=1804752281#gid=1804752281 Click for Process Control Charts] for GaAs etching.|link=https://docs.google.com/spreadsheets/d/16gHOO3PQn_LinrXGPeSTSBf5dnw3leSLh1gq0PLr43w/edit?gid=1804752281#gid=1804752281]]
*[https://docs.google.com/spreadsheets/d/16gHOO3PQn_LinrXGPeSTSBf5dnw3leSLh1gq0PLr43w/edit?gid=0#gid=0 GaAs Etch with N2/Cl2 - '''Etch Data''']
*[https://docs.google.com/spreadsheets/d/16gHOO3PQn_LinrXGPeSTSBf5dnw3leSLh1gq0PLr43w/edit?gid=1804752281#gid=1804752281 GaAs Etch with N2/Cl2 - '''Plots''']


==Photoresist and ARC etching (Panasonic 2)==
==Photoresist and ARC etching (Panasonic 2)==
Line 354: Line 456:
*Etch Rate for UV6-0.8 (DUV PR) = 518.5nm / 1min (2019, [[Demis D. John|Demis]])
*Etch Rate for UV6-0.8 (DUV PR) = 518.5nm / 1min (2019, [[Demis D. John|Demis]])
*2m30sec to fully remove UV6-0.8 with ~200% overetch (2019, [[Demis D. John|Demis]])
*2m30sec to fully remove UV6-0.8 with ~200% overetch (2019, [[Demis D. John|Demis]])
*Recipe #152 (Please revert when done)


==Ru (Ruthenium) Etch (Panasonic 2)==
==Ru (Ruthenium) Etch (Panasonic 2)==
Line 360: Line 463:
**''This etch is used in the following publication:'' [[Template:Publications#Highly Selective and Vertical Etch of Silicon Dioxide using Ruthenium Films as an Etch Mask|W.J. Mitchell, "Highly Selective and Vertical Etch of Silicon Dioxide using Ruthenium Films as an Etch Mask" (JVST-A, 2021)]]
**''This etch is used in the following publication:'' [[Template:Publications#Highly Selective and Vertical Etch of Silicon Dioxide using Ruthenium Films as an Etch Mask|W.J. Mitchell, "Highly Selective and Vertical Etch of Silicon Dioxide using Ruthenium Films as an Etch Mask" (JVST-A, 2021)]]


==SiO<sub>2</sub> Etching (Panasonic 2)==
=[[Oxford ICP Etcher (PlasmaPro 100 Cobra)]]=


===Recipes===
==Process Control Data (Oxford ICP Etcher)==


*[//wiki.nanotech.ucsb.edu/wiki/images/9/9e/33-Etching_SiO2_with_Vertical_Side-wall.pdf SiO<sub>2</sub> Vertical Etch Recipe#2 - CF<sub>4</sub>/CHF<sub>3</sub>]
===[https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit#gid=1804752281 Process Control Data for "Std InP Ridge Etch" Cl<sub>2</sub>/CH<sub>4</sub>/H<sub>2</sub>/60°C]===
**''This etch is used in our Process Control weekly cals run by [[Process Group Interns|NanoFab Interns]]. Very stable over time ±5%.''
''Calibration / Process testing data taken using the "InP Ridge Etch" process: Cl2/CH4/H2 @ 60°C, 1cm piece with ~50% SiO2 hardmask.''
*[//wiki.nanotech.ucsb.edu/wiki/images/1/1e/Panasonic2-ICP-Plasma-Etch-SiO2-nanoscale-rev1.pdf SiO<sub>2</sub> Nanoscale Etch Recipe - CHF<sub>3</sub>/O<sub>2</sub>]
*[//wiki.nanotech.ucsb.edu/wiki/images/d/d5/Panasonic2-SiOx-Recipe.pdf SiO<sub>2</sub> Vertical Etch Recipe - CHF<sub>3</sub> "SiOVert"]
**Direct copy of "SiOVert" from ICP#1, [[ICP_Etching_Recipes#SiO2_Etching_.28Panasonic_1.29|see parameters there]].


===Recipe Variations===
*[https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit?usp=sharing "Std InP Ridge Etch" Cl<sub>2</sub>/CH<sub>4</sub>/H<sub>2</sub>/60°C - '''Etch Data Tables''']
''Use these to determine how etch parameters affect the process.''
*[https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit#gid=1804752281 "Std InP Ridge Etch" Cl<sub>2</sub>/CH<sub>4</sub>/H<sub>2</sub>/60°C - '''Plots'''][[File:Oxford-ICP-Etch Process Control Data Example.jpg|alt=example SPC chart for Oxford ICP Etcher|none|thumb|225x225px|[https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit#gid=1804752281 Click for Process Control Charts]|link=https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit#gid=1804752281]]

*[https://wiki.nanotech.ucsb.edu/wiki/images/1/1e/05-SiO2_Nano-structure_Etch.pdf Angled SiO2 sidewall recipes]

===Process Control: SiO<sub>2</sub> Etch with CHF<sub>3</sub>/CF<sub>4</sub> (Panasonic 2)===
[[File:ICP2 Process Control Data Example.jpg|alt=example ICP2 process control chart|thumb|269x269px|[https://docs.google.com/spreadsheets/d/1m0l_UK2lDxlgww4f6nfXe4aQedNeDZsLs46jQ5wR4zw/edit#gid=1804752281 Click for Process Control Charts] for SiO<sub>2</sub> etching.|link=https://docs.google.com/spreadsheets/d/1m0l_UK2lDxlgww4f6nfXe4aQedNeDZsLs46jQ5wR4zw/edit#gid=1804752281]]''Weekly cal etches of the CF4/CHF3 SiO2 etch, run by [[Process Group Interns|NanoFab Interns]].''
*[https://docs.google.com/spreadsheets/d/1m0l_UK2lDxlgww4f6nfXe4aQedNeDZsLs46jQ5wR4zw/edit?usp=sharing SiO2 Etch with CHF3/CF4 - '''Etch Data''']
*[https://docs.google.com/spreadsheets/d/1m0l_UK2lDxlgww4f6nfXe4aQedNeDZsLs46jQ5wR4zw/edit#gid=1804752281 SiO2 Etch with CHF3/CF4 - '''Plots''']

==SiN<sub>x</sub> Etching (Panasonic 2)==

*[//wiki.nanotech.ucsb.edu/wiki/images/0/06/Panasonic2-ICP-Plasma-Etch-SiN-nanoscale-rev1.pdf SiN<sub>x</sub> Nanoscale Etch Recipe - CHF<sub>3</sub>/O<sub>2</sub>]

=[[Oxford ICP Etcher (PlasmaPro 100 Cobra)]]=

=== Process Tips ===
* Use the Santovac oil for mounting small pieces to Silicon carrier wafers, or else your resist will burn! Increases thermal conduction to the cooled carrier wafer. (Full-wafers instead get direct Helium cooling.) Careful that the oil does not get anywhere near the outer clamp that holds the wafer down, or your wafer will get stuck.
** The oil fully dissolves in Acetone or NMP. You can clean oil off the back by wiping the back of the sample against an ACE-soaked wipe.
* InP requires fairly high temperatures for making the Indium products volatile - so going to full-wafers (which are cooler) may requiring the table temperature. We have found that temperatures of ~150⁰C minimum may be required for preventing grassing etc.
* See the '''Process Control sections below''' - [[Process Group Interns|NanoFab Interns]] run Etches Weekly, tracked over time.
** This tells you whether the chamber and tool are operating properly before you run your etch.
** You can follow the intern's travelers for details of their etch.


==InP Ridge Etch (Oxford ICP Etcher)==
==InP Ridge Etch (Oxford ICP Etcher)==
===Low-Temp (60°C) Process===
===High-Temp (200°C) InP Etch Process===


*InP Ridge Etch 200°C - ''Noah Dutra & Fatt Foong, 2025-08-12''
**Etch rates ~2 um/min, Selectivity to SiO2 ~ 30:1, Sidewalls ~90°
**Very dependent on open area, more area => lower E.R.s
**Cal Sample: ~1cm sample etched with 1 quarter of blank 50mm InP seasoning wafer placed '''without''' mounting adhesive on blank Silicon carriers (rough side up).
**Recipe: Cl2/H2/Ar - 200°C

==== Process Control: High-Temp (200°C) InP Etch ====
[[File:200C InP.png|alt=example SPC chart for Oxford ICP Etcher|thumb|218x218px|[https://docs.google.com/spreadsheets/d/1LE5Cug9uJFYEwu0ZsNsp0W1dTRzcO2EKFhC0wu3w0n4/edit?gid=1804752281#gid=1804752281 Click for Process Control Charts] for 200°C InP Etch|link=https://docs.google.com/spreadsheets/d/1LE5Cug9uJFYEwu0ZsNsp0W1dTRzcO2EKFhC0wu3w0n4/edit?gid=1804752281#gid=1804752281]]''Calibration / Process testing data taken using the "InP Ridge Etch" process: Cl2/H2/Ar @ 200°C, 1cm piece with ~50% SiO2 hardmask.''
*[https://docs.google.com/spreadsheets/d/1LE5Cug9uJFYEwu0ZsNsp0W1dTRzcO2EKFhC0wu3w0n4/edit?gid=0#gid=0 "Std InP Ridge Etch" Cl<sub>2</sub>/H<sub>2</sub>/Ar 200°C - '''Etch Data Tables''']
*[https://docs.google.com/spreadsheets/d/1LE5Cug9uJFYEwu0ZsNsp0W1dTRzcO2EKFhC0wu3w0n4/edit?gid=1804752281#gid=1804752281 "Std InP Ridge Etch" Cl<sub>2</sub>/H<sub>2</sub>/Ar 200°C - '''Plots''']

===Low-Temp (60°C) InP Etch Process===
*[[Media:Oxford Etcher - InP Ridge Etch using Oxford PlasmaPro 100 Cobra - 2021-09-08.pdf|Low-Temp InP Ridge Etch Characterization]] - ''Ning Cao, 2021-09-08''
*[[Media:Oxford Etcher - InP Ridge Etch using Oxford PlasmaPro 100 Cobra - 2021-09-08.pdf|Low-Temp InP Ridge Etch Characterization]] - ''Ning Cao, 2021-09-08''
**<u>''No longer calibrating 60°C process as of 05-2025''.</u>
**InP etches were characterized with '''no''' mounting adhesive used, 1/4-wafer of 50mm wafer placed on blank Silicon carriers (rough side up).
**InP etches were characterized with '''no''' mounting adhesive used, 1/4-wafer of 50mm wafer placed on blank Silicon carriers (rough side up).
**Recipe: Cl2/CH4/H2 - 60°C
**Recipe: Cl2/CH4/H2 - 60°C
**NOTE: Rates in these 2021-09 characterizations are lower than current due to a software timing bug, fixed in 2022-01
**NOTE: Rates in these 2021-09 characterizations are lower than current due to a software timing bug, fixed in 2022-01
*See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning.
*See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning.

==== Process Control: Low-Temp (60°C) InP Etch ====
[[File:Oxford-ICP-Etch Process Control Data Example.jpg|alt=example SPC chart for Oxford ICP Etcher|thumb|225x225px|[https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit#gid=1804752281 Click for Process Control Charts] for 60°C InP Etch|link=https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit#gid=1804752281]]
2025-08-12: No longer run as weekly cal process, replaced by above 200°C Cl<sub>2</sub>/H<sub>2</sub>/Ar etch. Data below is for historical purposes only.
''Calibration / Process testing data taken using the "InP Ridge Etch" process: Cl2/CH4/H2 @ 60°C, 1cm piece with ~50% SiO2 hardmask.''

*[https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit?usp=sharing "Std InP Ridge Etch" Cl<sub>2</sub>/CH<sub>4</sub>/H<sub>2</sub>/60°C - '''Etch Data Tables''']
*[https://docs.google.com/spreadsheets/d/1cEUB7K5BAg9N4vp3rPZw7g0orFkxeQmRkX34Fb4eZco/edit#gid=1804752281 "Std InP Ridge Etch" Cl<sub>2</sub>/CH<sub>4</sub>/H<sub>2</sub>/60°C - '''Plots''']


====[[Oxford Etcher - Sample Size Effect on Etch Rate|Sample Size effect on Etch Rate]]====
====[[Oxford Etcher - Sample Size Effect on Etch Rate|Sample Size effect on Etch Rate]]====
Line 390: Line 538:
*See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning.
*See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning.


==GaAs Etch (Oxford ICP Etcher)==
== GaN Etch (Oxford ICP Etcher) ==
*''OLD 4" configuration: [https://drive.google.com/file/d/1B-Xg254T-RdALisnms0jvpJQ34i5TNXN/view?usp=drive_link Std GaN Etch - BCl3/Cl2/Ar - 200C Etch Characterization] - G.G.Meena, 2024-11-01''
This recipe also provides a starting point for '''GaSb'''-based etches.
**Etches characterized on ~1cmx1cm die, on 4<nowiki>''</nowiki> Si carrier wafer. Die has a SiN hard mask.
**Also includes explanation of the Taguchi (L9) DOE method for learning how process variables interact.
**[https://docs.google.com/spreadsheets/d/1QELHE6VUgq-xIfwIE50ddnsDtm7yfiOM/edit?usp=drive_link&ouid=103527106727572807737&rtpof=true&sd=true Etch development traveler with detailed characterization data]
**See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning.


==== Process Control: GaN Etch ====
*GaAs-based materials - etch recipe available on tool - ''provided by Oxford, not yet qualified internally''
CURRENT Recipe: ''6" STD GaN Etch - BCl3/Cl2/Ar - 200C (Public)'', on 1cm x 1cm with 6" configuration, ''~850nm deep GaN Etch with Cl2/BCl3/Ar at 200°C. GaN-on-Sapphire substrate with SiN mask.''
*See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning.


* This recipe is the same as the 4" (old) Std recipe but with 140% flows. Current recipe is 200c, 4.5mT, 700W/50W, Cl2/Ar/BCl3 = 49.1/16.4/11.6sccm.
==GaN Etch (Oxford ICP Etcher)==


* [https://docs.google.com/spreadsheets/d/1Pk8VwZlZ2lUf3aL9J2El5ZygqHY040TX3ZAMwa33LpE/edit?gid=0#gid=0 CURRENT 6" configuration: GaN Etching with Cl2/BCl3/Ar at 200°C - Etch Data]
*GaN-based materials - etch recipe available on tool - ''provided by Oxford, not yet qualified internally''
* [https://docs.google.com/spreadsheets/d/1Pk8VwZlZ2lUf3aL9J2El5ZygqHY040TX3ZAMwa33LpE/edit?gid=507237279#gid=507237279 CURRENT 6" configuration: GaN Etching with Cl2/BCl3/Ar at 200°C - Plots]
*See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning.

[[File:GaN SPC.png|alt=example of Process Control Charts|thumb|[https://docs.google.com/spreadsheets/d/1Pk8VwZlZ2lUf3aL9J2El5ZygqHY040TX3ZAMwa33LpE/edit?gid=507237279#gid=507237279 Click for Process Control Charts] for GaN Etch|link=https://docs.google.com/spreadsheets/d/1Pk8VwZlZ2lUf3aL9J2El5ZygqHY040TX3ZAMwa33LpE/edit?gid=507237279#gid=507237279|219x219px]]OLD Recipe: ''Std GaN Etch - BCl3/Cl2/Ar - 200C (Public)'', on 1cm x 1cm with 4" configuration, ''~1.2µm deep GaN etch with Cl2/BCl3/Ar at 200°C.'' ''GaN-on-Sapphire substrate with SiN mask.''
*[https://docs.google.com/spreadsheets/d/1Pk8VwZlZ2lUf3aL9J2El5ZygqHY040TX3ZAMwa33LpE/edit?gid=0#gid=0 OLD 4" configuration: GaN Etching with Cl2/BCl3/Ar at 200°C - Etch Data]
*[https://docs.google.com/spreadsheets/d/1Pk8VwZlZ2lUf3aL9J2El5ZygqHY040TX3ZAMwa33LpE/edit?gid=507237279#gid=507237279 OLD 4" configuration: GaN Etching with Cl2/BCl3/Ar at 200°C - Plots]
==GaAs Etch (Oxford ICP Etcher)==
*''[https://drive.google.com/file/d/1Q4pmX5M9v9dCD1xOg74kYguV12Szh9be/view?usp=drive_link Std GaAs Etch - BCl3/Ar - 20C Etch Characterization] - G.G.Meena, 2025-01-09''
**Etch characterization on 1cmx1cm die, on 4<nowiki>''</nowiki> Si carrier wafer. Die has SiO hard mask
**Also tested etch with PR mask.
**See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning
*''[https://wiki.nanofab.ucsb.edu/w/images/d/d1/GaAs_Etch_Ver3_Recipe_Finalized_120925.pdf Std GaAs Etch - Cl2/N2 - 30C Etch Characterization] - F. Foong, 2025-12-10''
**Etch characterization on 1cmx1cm die, on 4<nowiki>''</nowiki> Si carrier wafer. Die has SiO hard mask
**See [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Documentation|Operating Procedure]] for full traveler and post-cleaning


==GaN Atomic Layer Etching (Oxford ICP Etcher)==
==GaN Atomic Layer Etching (Oxford ICP Etcher)==

Revision as of 22:15, 23 September 2026

Back to Dry Etching Recipes.

DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)

Process Tips

  • Use the Santovac oil for mounting small pieces to Silicon carrier wafers, or else your resist will burn! Increases thermal conduction to the cooled carrier wafer. (Full-wafers instead get direct Helium cooling.) Careful that the oil does not get anywhere near the outer clamp that holds the wafer down, or your wafer will get stuck.
    • The oil fully dissolves in Acetone or NMP. You can clean oil off the back by wiping the back of the sample against an ACE-soaked wipe.
  • See the Process Control Data below - Staff/Intern-run Etches Weekly, tracked over time.
    • This tells you whether the chamber and tool are operating properly before you run your etch.
    • You can follow the intern's travelers for details of their etch.

Edge-Bead Removal (DSEiii)

Make sure to remove photoresist from edges of wafer, or PR may stick to the top-side wafer clamp and destroy your wafer during unload!

  • Edge Bead Removal via Photolithography: use a custom metal mask to pattern the photoresist with a flood exposure.
    • If you are etching fully through a wafer, remember that removal of edge-bead will cause full etching in the exposed areas. To prevent a wafer from falling into the machine after the etch, you can mount to a carrier wafer using wax.
  • Manual PR Edge-Bead Removal - using swabs and EBR100. This is prone to error and easy to accidentally leave a blob of PR on the edge - so be extra careful to ensure NO PR is left on the edges!

High Rate Bosch Etch (DSEIII)

  • Bosch Process Recipe and Characterization - Standard recipe on the tool.
    Example SEM image
    Example of 100µm Deep Bosch Etched Silicon posts with Al2O3 hard mask. Close inspection shows the horizontal "scalloping" from the cycling nature of the etch. (Image Credit: Demis D. John, 2021-07)
    • STD_Bosch_Si (⭐️Production) - Developed 2024-10
      • Old Recipe Name: "Plasma-Therm Standard DSE" - lower EtchA, less tolerant
    • Standard Bosch Process for high aspect-ratio, high-selectivity Silicon etching.
      • Cycles between polymer deposition "Dep" / Polymer etch "Etch A" / Si etch "Etch B" steps. Step Times gives fine control.
      • To reduce roughening/grassing ("black silicon"), Increase "Etch A" time by ~50%. Alternatively, reduce "Dep" step time by ~20%.
    • Patterns with different exposed/etched areas will have different "optimal" parameters.
    • This recipe has 2s Etch A time compared to "Plasma-Therm Standard DSE" (which has 1.5s Etch A) below - this reduced the undercut of mask to ~1% of the etch depth and the effect of aspect ratio on etch rate. All other recipe parameters are the same.
    • Selectivity to Photoresist ~60.
    • Selectivity to SiO2 should be higher, not yet measured.
    • Selectivity to Al2O3 is extremely high, >9000. See below TSV process for processing tips with Al2O3 hardmask.
    • If you need to pattern all the way to the edge of the wafer, PR won't work because you have to remove the edge-bead of photoresist (see above). Instead use hardmask process (See "Through Silicon Via" etch below).
    • Larger open area → lower selectivity & lower etch rate.
      • <1% center to edge variability in etch rate for small open area.
      • More variation across wafer for larger open area (eg. plasma dicing)
    • Thick PR's approx ≥10µm tend to burn, avoid thick PR's. They also make edge-bead removal very difficult. Instead use an SiO2 hardmask or the Al2O3/SiO2 hardmask below.
Tilted SEM of 40um deep etch
~40µm deep Silicon etch, run as Process Control "EtchCal" (Process Development and Image: Noah Dutra, 2024-10-07)
Example SEM image
Example of 16.32µm Deep Etched Silicon with 650nm thick UV6 Photoresist mask, 2µm Pitch. (Image Credit: Noah Dutra 2024-08)

Si Etching C4F8/SF6/Ar (PlasmaTherm DSEiii)

example of Process Control Charts
Click for Process Control Charts
  • Recipe: STD_Bosch_Si (⭐️Production), on 100mm Si Wafer with ~50% open area, photoresist mask, ~40µm deep

Through Silicon Via (TSV) etch (DSEiii)

Since the topside clamp requires the removal of photoresist on the outermost ~5-7mm of the wafer, this makes PR incompatible with through-silicon etching (as the outer edges would be etched-through, dropping the inner portion into the chamber). In addition, in practice we have found that thick PR often roughens and burns during long ~30-60min etches, making removal very difficult.

Instead, we recommend the following process with Al2O3 hardmask:

We have a new wafer-mounting process for through-silicon etching, using the UV-Release Dicing tape.  Contact staff for more info.
-- Demis 2026-02-10

NOTE: 
DO NOT RUN the wax-mounting process without discussing with staff first. The wax-mounting process process can leave wax on the wafer clamp, causing the next user's wafer to get stuck and fail transfer! 
(Through-wafer process with no wax is still acceptable.) -- Demis 2024-03-11
Process for Through-Wafer Silicon Etching

with wax-mounting (small pieces only)

Process to etch through ~550µm Silicon Demis D. John & Biljana Stamenic 2022-11-11. Please consider our publication policy if you use/modify this process.
Deposit 150nm Al2O3 on either: May need to do dep. rate check beforehand.
Deposit ~3nm SiO2, in situ (same machine as above) This improves adhesion to photoresist and prevents developer attacking the Al2O3.
Lithography - your preferred method. Needs approx. ≥500nm thick PR.
Etch the Al2O3 in Panasonic ICP 1/2 Use 50W version. Overetch by ~20%, will also etch through the thin SiO2 layer.
Strip PR - either in situ, or via NMP 80°C soak followed by PEii Technics ashing. In situ PR strip appears to give better + faster results.
If pieces of the wafer are at risk of falling into the chamber, mount the product wafer to a carrier wafer:

Logitech Wax Mounting Recipe - Bulk Crystal Bond


If you are only etching small holes through the wafer (majority of wafer is intact), then wax-mounting is not necessary.

CONTACT STAFF before attempting this step!


Critical - Ensure no wax is present on either side or edge of wafer prior to DSE etching, or wafer may break in the DSE during robot unload!

Use POLOS spinners with ACE/ISO to clean front and back of wafer.

IMPORTANT for wax-mounting, to ensure wax does not stick your wafer to the DSE clamp.

Observe carefully for any wax protruding from between wafers - redo spin-clean as needed.

Also make sure wax thickness is not too thick, of long etches could cause wax to seep out from between the wafers.
DSEiii etch - to eliminate grassing:
  • Increase EtchA LF-Bias Power and Duration
    • EtchA: 300W for 3.5–4sec
    • New method as of ~2025

Old method: reduce Dep step:

  • Bosch Cycles: Dep: 1.2sec / Etch A: 1.5sec / Etch B: 2.0sec
  • Rate ≈ 4.25µm / min
Can use Lasermonitor and/or Camera to observe when etch is fully through. Trenches may get black/rough, but then clear up when fully etched.
  • Record Helium FLOW during recipe run, for next step (if He leaks).
  • Ok to remove wafer, observe/measure, and re-load for etching.
  • If see black grass and etch rate drops, may need to run an O2 plasma with Technics PEii few min to remove polymer, Increase EtchA step time (eg. by 50-100%) and then continue the etch.
If you did not wax-mount your wafer, the recipe will eventually fail for Helium Pressure/Flow out of compliance. This is because the cooling Helium leaks through the wafer when the openings get fully etched through.

Once this happens,

  • Leave your wafer in the chamber, then
  • Edit recipe to set Helium Cooling (first step only) to "Flow Control Only".
  • Set to typical flow of normal process from above (Something like ~6sccm? Not sure. Exact value is not critical)
  • Re-run the recipe with He on Flow-control only until etch is complete.
Strip Al2O3/SiO2 either with Buffered HF, or same Pan1/2 dry etch as above.

BHF: Eg. ~2min to fully remove SiO2 + Al2O3, with overetch.

See etch BHF rates of the thin-films on this table.
IF wax-mounted - either
  • dissolve in Acetone overnight (make sure to excess-fill enough and cover tightly with tinfoil so it doesn't dry up), complete with ACE/ISO rinse

OR

  • place wafer on tinfoil-covered hotplate at 150°C, and slide product wafer off, then
    • ACE/ISO clean (eg. POLOS) to remove wax.
If you publish using the above process, please consider our publication policy. This process was developed by Biljana Stamenic and Demis D. John, 2022.

Plasma Dicing (DSEIII)

Coming Soon: Plasma Dicing process with Dicing Tape as backing film.

This process has been developed by staff, is currently in the final stages of finalizing a public recipe. Contact staff if you want to use it sooner.

Silicon: Single-Step, Low Etch Rate, Smooth Sidewall Process (DSEIII)

  • SF6-C4F8-CF4 Si Etch v1 (⭐️Production) - Developed 2026-01 by Noah Dutra
    • 12mT, 20/850W, C4F8/SF6/CF4=68.3/32.5/32.4sccm
    • E.R. = 339.4nm/min, Selectivity (to UV6) = 4.9
    • Smooth, Vertical, E.R. uniformity is within 5% on wafer
    • Tested with 4" wafers that are ~50% open with UV6 PR
  • Single Step Silicon Etch Recipe and Characterization
    • Older, alternate Si "shallow/smooth" etch recipe.
    • Recipe Name: "Nano Trench Etch" (Production - copy to your Personal category)
    • Used instead of Bosch Process, to avoid scalloping on the sidewall.
    • Lower selectivity, lower etch rate, smoother sidewalls.

SiO2 Etch (DSEiii)

These recipes were developed to serve as secondary pathways to the calibrated FICP SiO2 and Si etch calibrations here. Click here for SEMs comparing both cals.

  • CF4-C4F8 SiO2 Etch v1 (⭐️Production) - Developed 2026-01 by Noah Dutra
    • 3mT, 70/800W, C4F8/CF4=7.5/32.5sccm
    • E.R. = 270nm/min, Selectivity (to SPR955) = 1.3
    • Vertical/Smooth
    • Tested by mounting 1cmx1cm piece with oil on 4" Si

F-ICP Backup Recipes (DSEiii)

These recipes were developed to serve as backup processes for the calibrated Fluorine-ICP SiO2 and Si etches here.

Click here for SEMs comparing FICP to DSE etch processes.

PlasmaTherm/SLR Fluorine Etcher

Process Tips

  • Use the Santovac oil for mounting small pieces to Silicon carrier wafers, or else your resist will burn! Increases thermal conduction to the cooled carrier wafer. (Full-wafers instead get direct Helium cooling.) Careful that the oil does not get anywhere near the outer clamp that holds the wafer down, or your wafer will get stuck.
    • The oil fully dissolves in Acetone or NMP. You can clean oil off the back by wiping the back of the sample against an ACE-soaked wipe.
  • Process Control Data for this tool - Intern-run Etches Weekly, tracked over time.
    • SiO2 and Silicon etche performance is regularly tracked.
    • This tells you whether the chamber and tool are operating properly before you run your etch.
    • You can follow the intern's travelers for details of their etch.

Recipe Tips

  • RF1: Bias Power (with DCV readback)
  • RF2: ICP Power
  • For trouble igniting ICP plasma, add 15 to 75 W of bias power during ignition step. Typical ignition pressures 5 to 10 mT.

Si Etch Recipes (Fluorine ICP Etcher)

Example SEM image
Example of 1.65µm Deep Etched Silicon, 2µm Pitch. (Image Credit: Noah Dutra 2024-09)
  • "SiVertHFv2" (⭐️Production)
    • 20mTorr, RF=18W, ICP=950W, C4F8/SF6/CF4=120/48/54sccm
      • This recipe has 2x gas flow compared to "SiVertHF" below - this reduced the loading effect (dependence on % etched area).
    • Selectivity Silicon:Photoresist ≈ 5
    • Etch Rates: Si ≈ 300-350 nm/min; SiO2 ≈ 30-35 nm/min
    • 89-90 degree etch angle, ie, vertical.
    • High selectivity to Al2O3 masks.
      • For high aspect ratio Si etching, try ALD Al2O3 (~20-30nm) + SiO2 (2nm, for PR adhesion) hardmasks followed by Pan2 Al2O3 etch (will go straight through the thin SiO2 without additional etch time). Works well for allowing thin PR's (eg. DUV or EBL PR's) to enable deep etches.
    • Process Control Data below - Staff/Intern-run Etches Weekly, tracked over time (with no BARC layer).
  • Old Recipe: SiVertHF - Si Vertical Etch using C4F8/SF6/CF4 and resist mask

Process Notes/Observations

  • Due to high selectivity against SiO2, it may be necessary to run a ~10sec 50W SiO2 etch (below) to remove native oxide on Si. This can be performed in situ before the Si etch. It's possible this is actually an effect of photoresist open-area - we have conflicting results.
    • If you see very low etch rates, try the above SiO2 etch, or try a short PR/BARC etch.
  • We have observed that full-wafers with small open area in photoresist masks might require a recalibration of the C4F8/SF6 ratio in order to prevent very low etch rates.

Process Control: Si Etching C4F8/SF6/CF4 (Fluorine ICP Etcher)

example of Process Control Charts
Click for Process Control Charts

Full Wafer Si etching with ~50% open area and resist mask, run weekly by NanoFab Interns.

SiO2 Etch Recipes (Fluorine ICP Etcher)

SEM of FL-ICP 50W SiO2 etch with Ru Hard Mask
50W SiO2 Etch w/ Ru Hardmask
SEM of FL-ICP 200W SiO2 Etch with Ru Hardmask - Ning Cao
200W SiO2 Etch w/ Ru Hardmask (Ning Cao)
  • "SiO2 Etch-50W" (⭐️Production)
    • 3.8mT, RF=50W, ICP=900W, CHF3/CF4=10/30sccm
    • SiO2 etch rate: ~250nm/min
    • Selectivity SiO2:Photoresist ≈ 1.10–1.20
    • Selectivity SiO2:Ru ≈ 36
    • Process Control Data Above - Staff/Intern-run Etches Weekly, tracked over time.

SiO2 Etching using Ruthenium Hardmask

  • Click above for Full Process Traveler
    • Process written for Sputtered Ru & I-Line GCA Stepper litho
    • Can be transferred to ALD Ru or DUV/EBL Litho.
  • Ning Cao & Bill Mitchell, 2019-06
  • High-selectivity and deep etching using sputtered Ru hardmask and I-Line litho.
  • Etch also works well with PR masking
  • Chemistry: CHF3/CF4
  • Variations in SiO2 etch Bias Power: 50 / 200 / 400W bias.
  • Ru etch selectivity to PR: 0.18 (less than 1): 150nm Ru / 800nm PR
  • 50W Bias: (recommended)
    • Selectivity to photoresist: 1.10–1.20
    • SiO2 selectivity to Ru: 36
    • SiO2 etch rate: 263nm/min
    • Smoothest vertical etch for SiO2.
  • 200W Bias: (higher etch rate)
    • SiO2 selectivity to Ru: 38
    • SiO2 etch rate: 471nm/min
  • This etch is detailed in the following article: W.J. Mitchell et al., JVST-A, May 2021
  • Updates: Many users have found that SiO2-masking the Ru hardmask results in vastly improved photoresist selectivity, making litho+etch of small features much better.
    • Layer stack looks like: SiO2 (or other dielectric target layer to etch) / Ru hardmask / SiO2 hardmask (thin) / Photoresist.
    • Typically strip the masks+PR with all dry etching. That means the entire etch process (all etches and strips) can be run in situ on the Panasonic ICP in a rapid single-tool etch process.

Process Control: SiO2 Etching with CHF3/CF4 (Fluorine ICP Etcher)

example of Process Control Charts
Click for Process Control Charts

Full Wafer Si etching with ~50% open area and resist mask, run weekly by NanoFab Interns.

Si3N4 Etching (Fluorine ICP Etcher)

Developed by Bill Mitchell. Please see publication policy.

  • ICP = 950/75W
  • Pressure = 5mT
  • Low Polymer Dep: CF4 = 60sccm
    • Etch Rate = 420nm/min (PECVD Si3N4)
  • Higher verticality: CF4 = 35 / CHF3 = 25 sccm
    • Etch Rate = 380nm/min (PECVD Si3N4)

Photoresist & ARC (Fluorine ICP Etcher)

Chain multiple Recipes in a Flow, to allow you to to do in situ BARC etching, and follow up with in situ Photoresist Strip.

PR/BARC Etch (Fluorine ICP Etcher)

New PR Strip recipe: Wafer had UV6 or UVN30 as mask. 5min Si etch followed by PostBARC Etch/PR Strip (STD)_V2 with 2min over etch (Credit: Gopi Meena)
Old PR strip recipe: Wafer had UV6 or UVN30 as mask. 5min Si etch followed by PostBARC Etch/PR Strip (STD) with 2min over etch (Credit: Gopi Meena)
  • Etching DUV42P-6 Bottom Anti-Reflection Coating
    • ~60nm thick (2500krpm)
    • O2=20sccm / 10mT / RF1(bias)=100W / RF2(icp)=0W
    • 45sec-1min

Photoresist Strip/Polymer Removal (Fluorine ICP Etcher)

Old PR strip recipe: PostBARC Etch/PR Strip (STD)

  • O2=100sccm / 5mT / RF1(bias)=10W / RF2(icp)=825W
  • 75W Bias can be helpful for difficult to remove polymers, eg. 2min
  • Use laser monitor to check for complete removal, overetch to remove Fluorocarbon polymers.
  • Not able to completely remove PR (both negative & positive) after prolonged over etching (over etching of +2min)
  • Leaves behind residue on the sides

New PR strip recipe: PostBARC Etch/PR Strip (STD)_V2

  • O2=100sccm / 5mT / RF1(bias)=100W / RF2(icp)=825W
  • RF bias increased by 10x to 100W
  • Able to completely remove PR (both negative & positive) after over etching (over etching of +2min)
  • Clean surface with no residue

W Etching (Fluorine ICP Etcher)

W Etch. Image Credit: Fatt Foong

Developed by Fatt Foong. Please see publication policy.

  • ICP = 950/15W
  • Pressure = 10mT
  • C4F8/SF6/CF4 = 25/40/27sccm
    • Etch Rate = 128nm/min


Cleaning Procedures (Fluorine ICP Etcher)

ICP Etch 1 (Panasonic E646V)

Panasonic ICP#1 is currently down - Use Panasonic ICP#2 instead. Most processes directly transfer with only small change in etch rate. Data kept here for historical purposes only.

SiO2 Etching (Panasonic 1)

Recipes

Recipe Variations

Use these to determine how each etch parameter affects the process.

SiNx Etching (Panasonic 1)

Al Etch (Panasonic 1)

Cr Etch (Panasonic 1)

Ta Etch (Panasonic 1)

Ti Etch (Panasonic 1)

W-TiW Etch (Panasonic 1)

GaAs-AlGaAs Etch (Panasonic 1)

GaN Etch (Panasonic 1)

Photoresist and ARC Etching (Panasonic 1)

Please see the recipes for Panasonic ICP#2 - the same recipes apply.

Etching of DUV42P at standard spin/bake parameters also completes in 45 seconds.

SiC Etch (Panasonic 1)

Sapphire Etch (Panasonic 1)

Cleaning Recipes

To Be Added

Old Deleted Recipes

Since there are a limited number of recipe slots on the tool, we occasionally have to delete old, unused recipes.

If you need to free up a recipe slot, please contact the tool's Supervisor and they'll help you find an old recipe to replace. We take photographs of old recipes, and save them in case a group needs to revive the recipe. Contact us if your old recipe went missing.

Process Control Data (Panasonic 1)

SiO2 Etch with CHF3/CF4 - Process Control Data (Panasonic 1)

ICP Etch 2 (Panasonic E626I)

Recipes starting points for materials without processes listed can be obtained from Panasonic1 recipe files. The chambers are slightly different, but essentially the same, requiring only small program changes to obtain similar results.

Process Tips

  • Use the Santovac oil for mounting small pieces to Silicon carrier wafers, or else your resist will burn! Increases thermal conduction to the cooled carrier wafer. (Full-wafers instead get direct Helium cooling.) Careful that the oil does not get on the back of the carrier wafer or you will get Helium cooling errors.
    • The oil fully dissolves in Acetone or NMP. You can clean oil off the back by wiping the back of the sample against an ACE-soaked wipe.
  • See the Process Control sections below - NanoFab Interns run Etches Weekly, tracked over time.
    • This tells you whether the chamber and tool are operating properly before you run your etch.
    • You can follow the intern's travelers for details of their etch, and see their SEM's.

Al Etch (Panasonic 2)

Al2O3 Etching (Panasonic 2)

ALD Al2O3 Etch Rates in BCl3 Chemistry (click for plots of etch rate)

Contributed by Brian Markman, 2018

  • BCl3 = 30sccm
  • Pressure = 0.50 Pa
  • ICP Source RF = 500
  • Bias RF = 50W or 250W (250W can burn PR)
  • Cooling He Flow/Pressure = 15.0 sccm / 400 Pa
  • Etch Rate 50W: 39.6nm/min (0.66nm/sec)
  • Etch Rate 250W: 60.0nm/min (1.0 nm/sec)

Cr Etching (Panasonic 2)

  • Cl2=48, O2=12sccm, 1.33Pa, ICP=600W, RF=50W
    • Recipe #154 (please revert when done)
  • Handles larger area etching with less loading effect
  • Etch Rate: 24–33 nm/min
  • Use PR mask. selectivity not measured but ~500nm PR works easily for etching ~85nm Cr.
  • Strip PR in O2 plasma (in situ optional): Photoresist Etch/Strip (Panasonic 2)
  • Laser Monitor recommended

GaAs Etch (Panasonic 2)

Process Control: GaAs Etch with N2/Cl2 (Panasonic 2)

example ICP2 process control chart
Click for Process Control Charts for GaAs etching.

Photoresist and ARC etching (Panasonic 2)

Basic recipes for etching photoresist and Bottom Anti-Reflection Coating (BARC) underlayers are as follows:

ARC Etching: DUV-42P or AR6 (Panasonic 2)

  • O2 = 40 sccm // 0.5 Pa
  • ICP = 75W // RF = 75W
  • 45 sec for full etching (incl. overetch) of ~60nm DUV-42P (same as for AR6; 2018-2019, Demis/BrianT)

Photoresist Etch/Strip (Panasonic 2)

Works very well for photoresist stripping

  • O2 = 40 sccm // 1.0 Pa
  • ICP = 350W // RF = 100W
  • Etch Rate for UV6-0.8 (DUV PR) = 518.5nm / 1min (2019, Demis)
  • 2m30sec to fully remove UV6-0.8 with ~200% overetch (2019, Demis)
  • Recipe #152 (Please revert when done)

Ru (Ruthenium) Etch (Panasonic 2)

SiO2 Etching (Panasonic 2)

Recipes

Recipe Variations

Use these to determine how etch parameters affect the process.

Process Control: SiO2 Etch with CHF3/CF4 (Panasonic 2)

example ICP2 process control chart
Click for Process Control Charts for SiO2 etching.

Weekly cal etches of the CF4/CHF3 SiO2 etch, run by NanoFab Interns.

SiNx Etching (Panasonic 2)

Oxford ICP Etcher (PlasmaPro 100 Cobra)

Process Tips

  • Use the Santovac oil for mounting small pieces to Silicon carrier wafers, or else your resist will burn! Increases thermal conduction to the cooled carrier wafer. (Full-wafers instead get direct Helium cooling.) Careful that the oil does not get anywhere near the outer clamp that holds the wafer down, or your wafer will get stuck.
    • The oil fully dissolves in Acetone or NMP. You can clean oil off the back by wiping the back of the sample against an ACE-soaked wipe.
  • InP requires fairly high temperatures for making the Indium products volatile - so going to full-wafers (which are cooler) may requiring the table temperature. We have found that temperatures of ~150⁰C minimum may be required for preventing grassing etc.
  • See the Process Control sections below - NanoFab Interns run Etches Weekly, tracked over time.
    • This tells you whether the chamber and tool are operating properly before you run your etch.
    • You can follow the intern's travelers for details of their etch.

InP Ridge Etch (Oxford ICP Etcher)

High-Temp (200°C) InP Etch Process

  • InP Ridge Etch 200°C - Noah Dutra & Fatt Foong, 2025-08-12
    • Etch rates ~2 um/min, Selectivity to SiO2 ~ 30:1, Sidewalls ~90°
    • Very dependent on open area, more area => lower E.R.s
    • Cal Sample: ~1cm sample etched with 1 quarter of blank 50mm InP seasoning wafer placed without mounting adhesive on blank Silicon carriers (rough side up).
    • Recipe: Cl2/H2/Ar - 200°C

Process Control: High-Temp (200°C) InP Etch

example SPC chart for Oxford ICP Etcher
Click for Process Control Charts for 200°C InP Etch

Calibration / Process testing data taken using the "InP Ridge Etch" process: Cl2/H2/Ar @ 200°C, 1cm piece with ~50% SiO2 hardmask.

Low-Temp (60°C) InP Etch Process

  • Low-Temp InP Ridge Etch Characterization - Ning Cao, 2021-09-08
    • No longer calibrating 60°C process as of 05-2025.
    • InP etches were characterized with no mounting adhesive used, 1/4-wafer of 50mm wafer placed on blank Silicon carriers (rough side up).
    • Recipe: Cl2/CH4/H2 - 60°C
    • NOTE: Rates in these 2021-09 characterizations are lower than current due to a software timing bug, fixed in 2022-01
  • See Operating Procedure for full traveler and post-cleaning.

Process Control: Low-Temp (60°C) InP Etch

example SPC chart for Oxford ICP Etcher
Click for Process Control Charts for 60°C InP Etch
2025-08-12: No longer run as weekly cal process, replaced by above 200°C Cl2/H2/Ar etch. Data below is for historical purposes only.

Calibration / Process testing data taken using the "InP Ridge Etch" process: Cl2/CH4/H2 @ 60°C, 1cm piece with ~50% SiO2 hardmask.

Sample Size effect on Etch Rate

See the above table for data showing effect on sample size/exposed etched area.

InP Grating Etch (Oxford ICP Etcher)

  • InP/InGaAsP Grating Etch Characterization - Ning Cao, 2021-08-26
    • InP/InGaAsP etches were characterized with no mounting adhesive used, 1/4-wafer of 50mm wafer placed on Silicon carriers (rough side up).
    • Recipe: Cl2/CH4/H2/Ar - 20°C
    • NOTE: Rates in these 2021-09 characterizations are lower than current due to a software timing bug, fixed in 2022-01
  • See Operating Procedure for full traveler and post-cleaning.

GaN Etch (Oxford ICP Etcher)

Process Control: GaN Etch

CURRENT Recipe: 6" STD GaN Etch - BCl3/Cl2/Ar - 200C (Public), on 1cm x 1cm with 6" configuration, ~850nm deep GaN Etch with Cl2/BCl3/Ar at 200°C. GaN-on-Sapphire substrate with SiN mask.

  • This recipe is the same as the 4" (old) Std recipe but with 140% flows. Current recipe is 200c, 4.5mT, 700W/50W, Cl2/Ar/BCl3 = 49.1/16.4/11.6sccm.
example of Process Control Charts
Click for Process Control Charts for GaN Etch

OLD Recipe: Std GaN Etch - BCl3/Cl2/Ar - 200C (Public), on 1cm x 1cm with 4" configuration, ~1.2µm deep GaN etch with Cl2/BCl3/Ar at 200°C. GaN-on-Sapphire substrate with SiN mask.

GaAs Etch (Oxford ICP Etcher)

GaN Atomic Layer Etching (Oxford ICP Etcher)

GaN-ALE Recipe written and tested by users - contact supervisor for use.

Cleaning Recipes (Oxford ICP Etcher)

To Be Added: Required cleaning time & recipes