E-Beam 4 (CHA): Difference between revisions
| (39 intermediate revisions by 9 users not shown) | |||
| Line 1: | Line 1: | ||
{{ |
{{tool2|{{PAGENAME}} |
||
|picture=e-beam4.jpg |
|picture=e-beam4.jpg |
||
|type = Vacuum Deposition |
|type = Vacuum Deposition |
||
|super= |
|super= Michael Barreraz |
||
|super2= Bill Millerski |
|||
|phone=(805)839-3918x217 |
|||
|phone=(805)839-7975 |
|||
|location=Bay 3 |
|location=Bay 3 |
||
|email= |
|email=dfreeborn@ece.ucsb.edu |
||
|description = Multi-Wafer Evaporator |
|description = Multi-Wafer Evaporator |
||
|manufacturer = CHA Industries |
|manufacturer = CHA Industries |
||
| Line 11: | Line 12: | ||
|materials = |
|materials = |
||
|toolid=10 |
|toolid=10 |
||
}} |
}} |
||
[[File:EBeam4 Controls.jpeg|thumb|EBeam4's controls]] |
|||
= About = |
|||
This electron-beam evaporation system is the newest of the lab for metal deposition. This system is a bell-jar type system and has the capability to do up to 10-4” wafers in a lift-off configuration and up to 24-4” wafers in a sidewall coverage configuration. Rotational motion in combination with baffling is used for lift-off and provides roughly 5% uniformity across a 4” wafer. The sidewall coverage fixturing uses full planetary motion to provide coverage over all sidewalls. The system also an 8-pocket e-beam source and an Inficon IC/5 deposition controller that allows for programming of fully automated multiple layer depositions. The metals available for deposition are Al, Ti, Au, Pt, Ni, Pd, Ag, Ge, Fe, NiCr, NiFe and Cr. This system is used for n-type ohmic contact metalization to compound semiconductors, Schottky contacts to semiconductors, bond pads, and other general metalizations. The maximum deposition thickness during a run is limited to 1.0 microns. |
|||
== About == |
|||
= Detailed Specifications = |
|||
This electron-beam evaporation system is a bell-jar type system and has the capability to do up to 9-4” wafers in a lift-off configuration and up to 18-4” wafers in a sidewall coverage configuration. Rotational motion in combination with baffling is used for lift-off and provides roughly 5% uniformity across a 4” wafer. The system has an 8-pocket e-beam source and an Inficon IC/5 deposition controller that allows for programming of fully automated multiple layer depositions. |
|||
The sidewall coverage fixturing uses full planetary motion to provide coverage over all sidewalls. |
|||
The metals available for deposition are Al, Ti, Au, Pt, Ni, Pd, Ag, Ge, and Cr. |
|||
This system is used for n-type ohmic contact metalization to compound semiconductors, Schottky contacts to semiconductors, bond pads, and other general metalizations. |
|||
== Detailed Specifications == |
|||
*Temescal 10kV power supply |
*Temescal 10kV power supply |
||
*1-Temescal 8-pocket series 260 e-beam sources |
*1-Temescal 8-pocket series, 260 e-beam sources |
||
*Cryo-pumped system with ~ |
*Cryo-pumped system with ~ 5e-7 ultimate base pressure |
||
*Rotation with baffle for 5% uniformity over 4” wafer |
*Rotation with baffle for 5% uniformity over 4” wafer |
||
*Automatic vacuum sequencing |
*Automatic vacuum sequencing |
||
| Line 24: | Line 33: | ||
*Inficon IC/5 programmable crystal thickness monitoring system |
*Inficon IC/5 programmable crystal thickness monitoring system |
||
*Automatic deposition of multiple layer stacks |
*Automatic deposition of multiple layer stacks |
||
*Sample size: |
|||
*Sample size: Pieces or up to 10-4” wafers for lift-off and 24-4” wafers for sidewall coverage |
|||
**Pieces or |
|||
*Metals: Al, Ti, Au, Pt, Ni, Pd, Ag, Ge, Fe, NiCr, NiFe and Cr |
|||
**9x 4” wafers for lift-off (normal incidence) |
|||
**24x 4” wafers for sidewall coverage (planetary) |
|||
=Documentation= |
|||
**4x 6-inch wafers for normal incidence |
|||
*[[media:E-Beam-4-Operating-Procedures.pdf|Operating Procedures]] |
|||
*Metals: Al, Ti, Au, Pt, Ni, Pd, Ag, Ge, and Cr. |
|||
*Maximum deposition thickness during a run is limited to 1.0 microns. |
|||
= Materials Table = |
|||
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable" |
|||
|- |
|||
! colspan=6 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table</div> |
|||
|- bgcolor="#D0E7FF" |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Material''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Density, g/cm3''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Z Ratio''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Master tooling, %''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Process Gain, A/sec/%pwr''' |
|||
! width="100" bgcolor="#D0E7FF" align="center" | '''Comments''' |
|||
|- |
|||
|Ag |
|||
| 10.50 |
|||
| 0.529 |
|||
|110 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Al |
|||
| 2.70 |
|||
| 1.080 |
|||
|165 |
|||
|6.0 |
|||
| |
|||
|- |
|||
|Au |
|||
|19.30 |
|||
| 0.381 |
|||
|120 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Co |
|||
|8.90 |
|||
| 0.343 |
|||
|150 |
|||
|5.0 |
|||
| |
|||
|- |
|||
|Cr |
|||
|7.20 |
|||
| 0.305 |
|||
|140 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Fe |
|||
|7.86 |
|||
| 0.349 |
|||
|165 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Ge |
|||
|5.35 |
|||
| 0.516 |
|||
|126 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Hf |
|||
|13.09 |
|||
| 0.360 |
|||
|150 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Ir |
|||
|22.40 |
|||
| 0.129 |
|||
|130 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Ni |
|||
|8.91 |
|||
| 0.331 |
|||
|150 |
|||
|5.0 |
|||
| |
|||
|- |
|||
|NiCr |
|||
|8.23 |
|||
| 0.321 |
|||
|140 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|NiFe |
|||
|8.70 |
|||
|1.00 |
|||
|100 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Pd |
|||
|12.038 |
|||
|0.357 |
|||
|112 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Pt |
|||
|21.40 |
|||
|0.245 |
|||
|130 |
|||
|10.0 |
|||
| |
|||
|- |
|||
|Ru |
|||
|12.362 |
|||
|0.182 |
|||
|100 |
|||
|10.0 |
|||
| |
|||
|- |
|||
== Documentation == |
|||
*[https://wiki.nanofab.ucsb.edu/w/images/4/46/EB4_Operating_Instructions_6-6-24.pdf Operating Procedures] |
|||
*[https://wiki.nanofab.ucsb.edu/w/images/3/3a/EBeam4_Planetary_Fixture_SOP_1-29-26V45.47_Final.pdf Planetary Fixture SOP] (Requires SUM Reservation) |
|||
== Recipes == |
|||
=== Materials Table === |
|||
For tables listing all available materials and deposition parameters, please visit the [[E-Beam_Evaporation_Recipes#Materials_Table_(E-Beam #4)|'''E-Beam Recipe Page''']]. |
|||
=== Process Control Data === |
|||
| |
|||
*E-Beam 4 Ti: [https://docs.google.com/spreadsheets/d/1W7OFMAlRIcbpjm7FsbCh9ZLCCbhEp0bhtAC7UqEmJ5U/edit?gid=0#gid=0 Titanium Datasheet] & [https://docs.google.com/spreadsheets/d/1W7OFMAlRIcbpjm7FsbCh9ZLCCbhEp0bhtAC7UqEmJ5U/edit?gid=384597990#gid=384597990 Titanium Plots] |
|||
*E-Beam 4 Au: [https://docs.google.com/spreadsheets/d/1W7OFMAlRIcbpjm7FsbCh9ZLCCbhEp0bhtAC7UqEmJ5U/edit?gid=834604706#gid=834604706 Gold Datasheet] & [https://docs.google.com/spreadsheets/d/1W7OFMAlRIcbpjm7FsbCh9ZLCCbhEp0bhtAC7UqEmJ5U/edit?gid=721807140#gid=721807140 Gold Plots] |
|||
*E-Beam 4 Cr: [https://docs.google.com/spreadsheets/d/1W7OFMAlRIcbpjm7FsbCh9ZLCCbhEp0bhtAC7UqEmJ5U/edit?gid=1629968393#gid=1629968393 Chromium Datasheet] & [https://docs.google.com/spreadsheets/d/1W7OFMAlRIcbpjm7FsbCh9ZLCCbhEp0bhtAC7UqEmJ5U/edit?gid=701729811#gid=701729811 Chromium Plots] |
|||
*E-Beam 4 Ni: [https://docs.google.com/spreadsheets/d/1W7OFMAlRIcbpjm7FsbCh9ZLCCbhEp0bhtAC7UqEmJ5U/edit?gid=649905488#gid=649905488 Nickel Datasheet] & [https://docs.google.com/spreadsheets/d/1W7OFMAlRIcbpjm7FsbCh9ZLCCbhEp0bhtAC7UqEmJ5U/edit?gid=1525197973#gid=1525197973 Nickel Plots] |
|||
Latest revision as of 13:13, 30 September 2026
| ||||||||||||||||||||||||||||||||

About
This electron-beam evaporation system is a bell-jar type system and has the capability to do up to 9-4” wafers in a lift-off configuration and up to 18-4” wafers in a sidewall coverage configuration. Rotational motion in combination with baffling is used for lift-off and provides roughly 5% uniformity across a 4” wafer. The system has an 8-pocket e-beam source and an Inficon IC/5 deposition controller that allows for programming of fully automated multiple layer depositions.
The sidewall coverage fixturing uses full planetary motion to provide coverage over all sidewalls.
The metals available for deposition are Al, Ti, Au, Pt, Ni, Pd, Ag, Ge, and Cr.
This system is used for n-type ohmic contact metalization to compound semiconductors, Schottky contacts to semiconductors, bond pads, and other general metalizations.
Detailed Specifications
- Temescal 10kV power supply
- 1-Temescal 8-pocket series, 260 e-beam sources
- Cryo-pumped system with ~ 5e-7 ultimate base pressure
- Rotation with baffle for 5% uniformity over 4” wafer
- Automatic vacuum sequencing
- Temescal e-beam sweep control
- Inficon IC/5 programmable crystal thickness monitoring system
- Automatic deposition of multiple layer stacks
- Sample size:
- Pieces or
- 9x 4” wafers for lift-off (normal incidence)
- 24x 4” wafers for sidewall coverage (planetary)
- 4x 6-inch wafers for normal incidence
- Metals: Al, Ti, Au, Pt, Ni, Pd, Ag, Ge, and Cr.
- Maximum deposition thickness during a run is limited to 1.0 microns.
Documentation
- Operating Procedures
- Planetary Fixture SOP (Requires SUM Reservation)
Recipes
Materials Table
For tables listing all available materials and deposition parameters, please visit the E-Beam Recipe Page.
Process Control Data
- E-Beam 4 Ti: Titanium Datasheet & Titanium Plots
- E-Beam 4 Au: Gold Datasheet & Gold Plots
- E-Beam 4 Cr: Chromium Datasheet & Chromium Plots
- E-Beam 4 Ni: Nickel Datasheet & Nickel Plots